Preparation method and application of graphene-coated single-particle nanodiamond material

The preparation method of graphene-coated single-particle nanodiamond material solves the problems of nanodiamond purity and dispersion, and improves the cycle stability and performance of lithium-ion batteries.

CN118145639BActive Publication Date: 2024-11-15GUANGDONG QIXIAN SMART FURNITURE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410256345.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-06
Publication Date
2024-11-15
Estimated Expiration
2044-03-06

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare high-purity, single-particle nanodiamonds, and existing processing methods may introduce impurities, affecting their application in lithium-ion batteries.

Method used

A formulation and preparation method for graphene-coated single-particle nanodiamond materials were developed. Nanodiamonds were prepared by detonation and surface modification was performed under ultrasonic and ultraviolet irradiation to avoid the introduction of metal ions or sulfate ions, thus ensuring purification effect and improving dispersibility.

Benefits of technology

The prepared nanodiamond material is uniformly dispersed in lithium-ion batteries, providing more storage sites, improving the rapid adsorption and desorption of lithium ions, and enhancing the cycle stability of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of chemical materials, and provides a formula and preparation method of a graphene-coated single-particle nano-diamond material, wherein the formula of the graphene-coated single-particle nano-diamond material includes the following raw materials by mass fraction: Co1-5%, Ni2-3%, La1-3%, Cu0.3-0.8%, Cr5-7%, trinitrotoluene 50-55%, and cyclotrimethylene trinitramine makes up the surplus. The nano-diamond particles prepared by the detonation method of the present invention have fewer defects on the surface and are easier to purify. At the same time, the ultrasonic dispersion conditions of the present invention do not introduce impurities such as metal ions or sulfate ions or chloride ions, thereby ensuring the effect of purification. The nano-diamond material prepared by the present invention can achieve deagglomeration and stable dispersion in commercially available electrolytes, provide more storage sites for lithium ions, improve the rapid adsorption and desorption capabilities of lithium ions, and achieve the improvement of the cycle stability of lithium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical materials, and specifically relates to a formula and a preparation method of a graphene-coated single-particle nanodiamond material. Background Art

[0002] In 1963, Soviet scientists discovered that nanodiamonds, also known as ultra-dispered diamonds (UDD), can be produced from nuclear explosions produced by carbon-based explosives. Since then, people have begun to use the detonation method to prepare this material with great application prospects. Although nanodiamonds can also be obtained by processes such as hydrothermal synthesis, ion bombardment, and microwave plasma chemical vapor deposition technology, the detonation method is faster, more efficient, and energy-saving than them. It has now become one of the main industrial production methods for nanodiamonds.

[0003] The preparation method of detonation nanodiamond is to mix trinitrotoluene with detonation property and cyclotrimethylene trinitramine as white crystalline non-water-soluble detonation component in a specified ratio. When the above-mentioned mixed detonation substances react, in the instantaneous high temperature and high pressure atmosphere, the carbon component of the composition generates a diamond crystal nucleus (SP3 structure of carbon), the above-mentioned nucleus grows to a specified size, and there are single and multiple functional groups composed of C, O, H and N on the surface of graphite (SP2 structure). Since the detonation reaction process of detonation nanodiamond is very short, and shrinkage occurs at the same time as the detonation, the phenomenon of strong aggregation of multiple single diamond particles generated has the disadvantage that it is not only difficult to separate into single particles or multiple particle clusters, but also difficult to purify the impurities contained in the above-mentioned aggregated diamond particles. In the prior art, the purification process usually uses acids (for example, sulfuric acid, hydrochloric acid, potassium permanganate, etc.) or strong bases that have the hidden danger of impurities being mixed in, and there is also the problem of metal impurities being mixed in the purification process. Therefore, there is an urgent need for a method for preparing high-purity, single-particle nanodiamonds.

[0004] As a new type of green energy, lithium-ion batteries are widely used in electric vehicles, mobile phones, computers and other fields. The positive electrode material of lithium-ion batteries directly affects the key performance of the battery, such as safety, energy density, and processability. However, the cycle stability of existing lithium-ion batteries is not ideal and cannot meet people's increasingly high requirements for battery energy density. Improving the cycle stability and temperature resistance of lithium-ion batteries is also an urgent problem to be solved. Summary of the invention

[0005] The purpose of the present invention is to provide a formula and preparation method of a graphene-coated single-particle nanodiamond material. The nanodiamond prepared by the present invention has good dispersion and high purity. After being added to a commercially available electrolyte, it can provide more active sites, and the cycle stability of a lithium battery prepared therein can be improved.

[0006] In order to achieve the above-mentioned purpose, the present invention provides the following technical scheme: a formula of a graphene-coated single-particle nanodiamond material, comprising the following raw materials in mass fractions: Co1-5%, Ni2-3%, La1-3%, Cu0.3-0.8%, Cr5-7%, trinitrotoluene 50-55%, and cyclotrimethylene trinitramine making up the balance.

[0007] Furthermore, the raw materials include the following mass fractions: Co 3.4%, Ni 2.5%, La 2.6%, Cu 0.5%, Cr 6.2%, trinitrotoluene 52%, and cyclotrimethylene trinitramine making up the balance.

[0008] The present invention also provides a method for preparing a graphene-coated single-particle nanodiamond material, comprising the following steps:

[0009] (1) Weigh the raw materials according to the formula, mix and stir evenly, and press the raw materials into a shape consistent with the shape of the cavity inside the reaction container, with a density of 3-5 tons / m 2 , the volume ratio of the reaction vessel to the internal cavity volume is 1:60-65;

[0010] (2) loading the raw materials into a reaction container, wherein the reaction container is in a nitrogen environment, and using a detonator to trigger the raw materials to react to synthesize reaction products;

[0011] (3) Mix the reaction product and deionized water in a mass ratio of 1:10-13, heat to 85°C and stir for 30-40 minutes, continue to add ethanol in an amount equal to the volume of deionized water, adjust the pH to 9 with NH4OH, and perform ultrasonic treatment at 2.5-3kHz for 2.4-2.6 hours; use a high-speed centrifugal device at a speed of 25,000 rpm for 50-100 seconds to obtain ultrasonically treated nanodiamonds;

[0012] (4) The ultrasonically treated nanodiamond is heated at 1200°C for 1.5-2h in a nitrogen atmosphere; and then treated under ultraviolet UV irradiation for 30-40s to obtain a graphene-coated single-particle nanodiamond material.

[0013] Furthermore, the ultraviolet UV irradiation lamp is 250W.

[0014] Furthermore, the graphene-coated single-particle nanodiamond material has a particle size of 2 to 5 nm.

[0015] Furthermore, the density is 4 tons / m 2 .

[0016] Furthermore, the volume ratio to the volume of the internal cavity of the reaction container is 1:62.

[0017] Furthermore, the ultrasound was performed at 2.8 kHz for 2.5 h.

[0018] Further, the reaction product was mixed with deionized water in a mass ratio of 1:12.

[0019] Further, the mixture was heated to 85°C and stirred for 35 min.

[0020] Nanodiamonds prepared by detonation method have the dual characteristics of diamond and nanomaterials. They not only have the ultra-high hardness, good chemical stability and wear resistance of diamond, but also have the unique characteristics of nanomaterials such as large specific surface area and quantum effect. Their thermal, magnetic, optical and electrical properties are different from those of normal particles, which makes them widely used in mechanical processing, optics, biology, medicine and other fields. Adding nanodiamonds to the electrolyte system has also become an important way to improve the cycle performance of batteries. The use of nanodiamonds can increase the adsorption of lithium, improve the reversible capacity and lithium ion transfer rate. It has received more and more attention in the application field of lithium-ion batteries. However, the cycle stability performance of batteries prepared using commercially available nanodiamonds is not ideal, especially the cycle stability under high and low temperatures directly limits the application of nanodiamonds in batteries.

[0021] The nano-diamond particles prepared by the detonation method of the present invention have fewer defects on the surface and are easier to purify. However, due to the large specific surface area of ​​nano-diamonds, there are more functional groups adsorbed on the surface, and the existing treatment methods usually use reagents for acidification, oxidation, and alkalization, which may lead to the introduction of impurity metals, adsorption of sulfate ions or chloride ions on the surface of nano-diamonds. The presence of the above functional groups changes the surface potential of nano-diamonds, causing nano-diamond particles to agglomerate, thereby causing the excellent properties of nano-diamonds to be unable to be fully utilized, which seriously limits the application of nano-diamonds in electrolyte systems. The ultrasonic dispersion conditions of the present invention do not introduce metal ions, sulfate ions, chloride ions, etc., which ensures the purification effect and improves the dispersibility.

[0022] Furthermore, the graphene coated on the surface of the nano-diamond obtained by the detonation method is not uniform. The present invention modifies the surface of the nano-diamond material after ultrasonic dispersion, firstly calcining the nano-diamond surface at high temperature to coat the graphene for the second time, and then irradiating it with ultraviolet light to obtain the final product, the graphene-coated single-particle nano-diamond material. The nano-diamond material obtained by the present invention can be deagglomerated and stably dispersed in commercially available electrolytes, providing more storage sites for lithium ions, improving the rapid adsorption and desorption capabilities of lithium ions, and achieving the improvement of the cycle stability of lithium-ion batteries.

[0023] Compared with the prior art, the advantages and beneficial effects of the present invention are:

[0024] 1. The purpose of the present invention is to provide a formula and preparation method of a graphene-coated single-particle nanodiamond material. The nanodiamond prepared by the present invention has high dispersion and is evenly dispersed when added to a commercially available electrolyte. The preparation of a lithium battery can improve the cycle stability.

[0025] 2. The nano-diamond particles prepared by the detonation method of the present invention have fewer surface defects and are easier to purify. The ultrasonic dispersion conditions of the present invention do not introduce metal ions, sulfate ions, chloride ions, etc., thus ensuring the purification effect.

[0026] 3. The nano-diamond material prepared by the present invention can be deagglomerated and stably dispersed in commercially available electrolytes, providing more storage sites for lithium ions, improving the rapid adsorption and desorption capabilities of lithium ions, and achieving improved cycle stability of lithium-ion batteries. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] This embodiment provides a formula for a graphene-coated single-particle nanodiamond material, including the following raw materials in mass fractions: Co3.4%, Ni2.5%, La2.6%, Cu0.5%, Cr6.2%, trinitrotoluene 52%, and cyclotrimethylene trinitramine to make up the balance.

[0030] The method for preparing the graphene-coated single-particle nanodiamond material comprises the following steps:

[0031] (1) Weigh the raw materials according to the formula, mix and stir evenly, and press the raw materials into a shape consistent with the shape of the cavity inside the reaction container. The density is 4 tons / m2 , the volume ratio of the reaction vessel to the internal cavity volume is 1:62;

[0032] (2) loading the raw materials into a reaction container, wherein the reaction container is in a nitrogen environment, and using a detonator to trigger the raw materials to react to synthesize reaction products;

[0033] (3) Mix the reaction product and deionized water in a mass ratio of 1:12, heat to 85°C and stir for 35 minutes, continue to add ethanol in an equal volume to the deionized water, adjust the pH to 9 with NH4OH, and perform ultrasonic treatment at 2.8kHz for 2.5 hours; use a high-speed centrifuge at a speed of 25,000 rpm for 70 seconds to obtain ultrasonically treated nanodiamonds;

[0034] (4) The ultrasonically treated nanodiamond was heated at 1200° C. for 1.7 h in a nitrogen atmosphere; and then treated under ultraviolet UV irradiation for 35 s, wherein the ultraviolet UV irradiation lamp was 250 W, to obtain a graphene-coated single-particle nanodiamond material.

[0035] The particle size of the graphene-coated single-particle nanodiamond material is 2-5 nm.

[0036] Example 2

[0037] This embodiment provides a formula for preparing a graphene-coated single-particle nanodiamond material, including the following raw materials in mass fractions: Co3.4%, Ni2.5%, La2.6%, Cu0.5%, Cr6.2%, trinitrotoluene 52%, and cyclotrimethylene trinitramine to make up the balance.

[0038] The method for preparing the graphene-coated single-particle nanodiamond material comprises the following steps:

[0039] (1) Weigh the raw materials according to the formula, mix and stir evenly, and press the raw materials into a shape consistent with the shape of the cavity inside the reaction container. The density is 4 tons / m 2 , the volume ratio of the reaction vessel to the internal cavity volume is 1:62;

[0040] (2) loading the raw materials into a reaction container, wherein the reaction container is in a nitrogen environment, and using a detonator to trigger the raw materials to react to synthesize reaction products;

[0041] (3) Mix the reaction product and deionized water in a mass ratio of 1:13, heat to 85°C and stir for 30 min, continue to add ethanol in an equal volume to the deionized water, adjust the pH to 9 with NH4OH, and perform ultrasonic treatment at 2.5 kHz for 2.6 h; use a high-speed centrifuge at a speed of 25,000 rpm for 90 seconds to obtain ultrasonically treated nanodiamonds;

[0042] (4) The ultrasonically treated nanodiamond was heated at 1200° C. for 1.5 h in a nitrogen atmosphere; and then treated under ultraviolet UV irradiation for 30 s, wherein the ultraviolet UV irradiation lamp was 250 W, to obtain a graphene-coated single-particle nanodiamond material.

[0043] The particle size of the graphene-coated single-particle nanodiamond material is 2-5 nm.

[0044] Comparative Example 1

[0045] The difference between this comparative example and Example 1 is that step (3) is different.

[0046] Specifically: This comparative example provides a formula of graphene-coated single-particle nanodiamond material, including the following raw materials in mass fractions: including the following raw materials in mass fractions: Co3.9%, Ni2.4%, La1.9%, Cu0.8%, Cr6.7%, trinitrotoluene 52%, and cyclotrimethylene trinitramine making up the balance.

[0047] The method for preparing the graphene-coated single-particle nanodiamond material comprises the following steps:

[0048] (1) Weigh the raw materials according to the formula, mix and stir evenly, and press the raw materials into a shape consistent with the shape of the cavity inside the reaction container. The density is 4 tons / m 2 , the volume ratio of the reaction vessel to the internal cavity volume is 1:62;

[0049] (2) loading the raw materials into a reaction container, wherein the reaction container is in a nitrogen environment, and using a detonator to trigger the raw materials to react to synthesize reaction products;

[0050] (3) at room temperature and pressure, the reaction product with a mass ratio of 1:15 was mixed with dilute hydrochloric acid with a concentration of 25 wt%, acidified for 2 hours, filtered and washed, and the washed reaction product with a mass ratio of 1:15 was mixed with sodium hydroxide with a concentration of 30 wt% at room temperature and pressure, alkalized for 3 hours, filtered and washed, to obtain acid-base treated nanodiamonds;

[0051] (4) The acid-base treated nanodiamond was heated at 1200° C. for 1.7 h in a nitrogen atmosphere; and then treated under ultraviolet UV irradiation for 35 s, wherein the ultraviolet UV irradiation lamp was 250 W, to obtain a graphene-coated single-particle nanodiamond material.

[0052] The graphene-coated single-particle nanodiamond material has a particle size of 5 to 10 nm.

[0053] Comparative Example 2

[0054] The difference between this comparative example and Example 1 is that step (4) is different.

[0055] Specifically: This comparative example provides a formula of a graphene-coated single-particle nanodiamond material, including the following raw materials in mass fractions: Co3.4%, Ni2.5%, La2.6%, Cu0.5%, Cr6.2%, trinitrotoluene 52%, and cyclotrimethylene trinitramine to make up the balance.

[0056] The method for preparing the graphene-coated single-particle nanodiamond material comprises the following steps:

[0057] (1) Weigh the raw materials according to the formula, mix and stir evenly, and press the raw materials into a shape consistent with the shape of the cavity inside the reaction container. The density is 4 tons / m 2 , the volume ratio of the reaction vessel to the internal cavity volume is 1:62;

[0058] (2) loading the raw materials into a reaction container, wherein the reaction container is in a nitrogen environment, and using a detonator to trigger the raw materials to react to synthesize reaction products;

[0059] (3) Mix the reaction product and deionized water in a mass ratio of 1:12, heat to 85°C and stir for 35 minutes, continue to add ethanol in an equal volume to the deionized water, adjust the pH to 9 with NH4OH, and perform ultrasonic treatment at 2.8kHz for 2.5 hours; use a high-speed centrifuge at a speed of 25,000 rpm for 70 seconds to obtain ultrasonically treated nanodiamonds;

[0060] (4) The nanodiamond treated with ultrasound was treated under ultraviolet UV irradiation for 15 seconds, and the ultraviolet UV irradiation lamp was 250W to obtain a graphene-coated single-particle nanodiamond material.

[0061] The particle size of the graphene-coated single-particle nanodiamond material is 2-5 nm.

[0062] Comparative Example 3

[0063] Commercially available nanodiamond material was purchased from Merck, catalog number: 900180.

[0064] Performance Testing

[0065] 1. Prepare lithium-ion batteries according to the following steps:

[0066] (1) The nano-diamond materials prepared in Examples 1-2 and Comparative Examples 1-3 were added to a commercial LiPF6 (ethylene carbonate: dimethyl carbonate = 1:1) electrolyte and subjected to ultrasonic treatment for 20 min under argon protection to obtain a nano-diamond electrolyte with a nano-diamond concentration of 0.5 mg / mL;

[0067] (2) The graphite negative electrode, carbon black, thickener (CMC), and adhesive (SBR) are uniformly mixed in a mass ratio of 95.2:1:1.9:1.9, slurried, coated, and rolled, and then coated on a copper foil, dried at 120°C, cut into an electrode shape, and compacted to obtain a negative electrode for a lithium-ion battery;

[0068] (3) In an environment without water or oxygen, a battery is formed with metallic lithium as the positive electrode, the electrolyte being nano-diamond electrolyte and the negative electrode being a lithium-ion battery.

[0069] 2. The battery prepared by the above method is subjected to performance test:

[0070] 1. Battery room temperature cycle performance test: At 25°C, the battery is charged to 4.2V at 0.5C constant current and constant voltage, with a cut-off current of 0.05C, and then discharged to 3.0V at 0.5C constant current. After 500 cycles of charge / discharge, the capacity retention rate of the 500th cycle is calculated. The calculation formula is as follows: 500th cycle capacity retention rate (%) = (500th cycle discharge capacity / first cycle discharge capacity) × 100%.

[0071] 2. Battery high temperature test: Place the battery at room temperature and charge and discharge it once at 0.5C (4.2V~3.0V), record the battery discharge capacity C0 before storage, then charge the battery with constant current and constant voltage to 4.2V full charge state, then store the battery in a 45℃ constant temperature box for 7 days, after the battery cools at room temperature for 24h, discharge the battery again at 0.5C constant current to 3.0V, record the battery discharge capacity C1 after storage, and calculate the battery capacity remaining rate after 7 days of constant temperature storage at 45℃. The calculation formula is as follows: Capacity remaining rate after 7 days of constant temperature storage at 45℃ = C1 / C0*100%.

[0072] 3. Battery low temperature test: Place the battery at room temperature and charge and discharge it once at 0.5C (4.2V~3.0V), record the battery discharge capacity C2 before storage, and then charge the battery to 4.2V full charge state with constant current and constant voltage. Place the battery in a low temperature box. When the temperature of the low temperature box drops to -40℃, leave it for 4 hours, and then discharge the battery to 3.0V at 0.5C constant current, record the battery discharge capacity C3 after storage, and calculate the -40℃ constant current discharge ratio. The calculation formula is as follows: -40℃ constant current discharge ratio = C3 / C2*100%.

[0073] Table 1 Performance test results

[0074] 25℃ first cycle discharge capacity mA·h / g 25℃ Cycle Test% High temperature cycle test% Low temperature cycle test% Example 1 546 98.7 98.5 94.3 Example 2 541 98.5 98.2 94.0 Comparative Example 1 505 92.6 85.7 82.1 Comparative Example 2 484 93.6 82.6 81.5 Comparative Example 3 437 86.8 65.6 61.4

[0075] It can be seen from Examples 1-2 that the battery prepared with the nano-diamond material prepared by the present invention not only has an excellent cycle capacity retention rate at room temperature, but also has excellent performance at high and low temperatures, which broadens the use of lithium-ion batteries under different conditions and is of great significance to the development of lithium batteries. It is significantly better than the nano-diamond materials on the market. And it can be seen from Comparative Examples 1-3 that the performance of the battery decreases to varying degrees by changing the preparation conditions of the nano-diamond material of the present invention.

[0076] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A use of graphene-coated single-particle nanodiamond in improving the cycle stability of lithium batteries, wherein the graphene-coated single-particle nanodiamond comprises the following raw materials by mass fraction: Co1-5%, Ni2-3%, La1-3%, Cu0.3-0.8%, Cr5-7%, trinitrotoluene 50-55%, and cyclotrimethylene trinitramine makes up the balance; The method for preparing graphene-coated single-particle nanodiamond comprises the following steps: (1) Weigh the raw materials according to the formula, mix and stir evenly, and press the raw materials into a shape consistent with the shape of the cavity inside the reaction container, with a density of 3-5 tons / m 2 , the volume ratio of the reaction vessel to the internal cavity volume is 1:60-65; (2) loading the raw materials into a reaction container, wherein the reaction container is in a nitrogen environment, and using a detonator to trigger the raw materials to react to synthesize a reaction product; (3) mixing the reaction product and deionized water at a mass ratio of 1:10-13, heating to 85° C. and stirring for 30-40 min, adding an equal volume of ethanol to the deionized water, adjusting the pH to 9 with NH4OH, and performing ultrasonic treatment at 2.5-3kHz for 2.4-2.6 h; using a high-speed centrifugal device at a speed of 25,000 rpm for 50-100 seconds to obtain ultrasonically treated nanodiamonds; (4) heating the ultrasonically treated nanodiamond at 1200° C. for 1.5-2 h in a nitrogen atmosphere; and then treating it under ultraviolet UV irradiation for 30-40 s to obtain a graphene-coated single-particle nanodiamond; The UV irradiation lamp in step (4) is 250W; In the step (4), the particle size of the graphene-coated single-particle nanodiamond is 2 to 5 nm.

2. The use of the graphene-coated single-particle nanodiamond according to claim 1 in improving the cycle stability of lithium batteries, characterized in that: The density in step (1) is 4 tons / m 2 .

3. The use of the graphene-coated single-particle nanodiamond according to claim 1 in improving the cycle stability of lithium batteries, characterized in that: The ratio of the volume in step (1) to the volume of the internal cavity of the reaction container is 1:

62.

4. The use of the graphene-coated single-particle nanodiamond in improving the cycle stability of lithium batteries according to claim 1, characterized in that: In the step (3), the ultrasonic wave is applied at 2.8 kHz for 2.5 hours.

5. The use of the graphene-coated single-particle nanodiamond in improving the cycle stability of lithium batteries according to claim 1, characterized in that: The reaction product in step (3) is mixed with deionized water in a mass ratio of 1:

12.

6. The use of the graphene-coated single-particle nanodiamond in improving the cycle stability of lithium batteries according to claim 1, characterized in that: In the step (3), the mixture is heated to 85° C. and stirred for 35 min.