Ultra-high strength, high toughness steel and its preparation method and application
By adding elements such as vanadium and niobium to steel, and using low-frequency pulse current and electromagnetic fields for magnetic plastic processing, the problems of high deformation resistance and poor processing performance of high-strength and high-toughness steel during processing and forming are solved, and ultra-high strength is achieved , high toughness and high plasticity, reducing mold damage and extending mold life.
Patent Information
- Application Number
- CN202410143607.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-01
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-02-01
AI Technical Summary
Existing high-strength and high-toughness steels have problems such as high deformation resistance and poor processing performance during processing and forming. It is difficult to achieve high strength, high plasticity and ease of processing at the same time.
Specific contents of vanadium (V) and niobium (Nb) are added to the steel, combined with Mn, Cu, Al, Ni, and C, and the impact effect and electromagnetic field generated by low-frequency pulse current are used for magnetic plasticity processing to reduce the yield strength and promote phase change. Variation-induced plasticity effect, improve the strong plasticity of steel, and improve the strength and plasticity of steel through the principles of precipitation strengthening and grain refinement.
The realization of ultra-high strength, high toughness, and high plasticity steel reduces the quality requirements for the mold and the damage to the mold during processing, improves the processing performance, and extends the service life of the mold.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of alloys, and in particular relates to an ultra-high strength and high toughness steel and a preparation method and application thereof. Background Art
[0002] With the growing demand for lightweight and safety in aerospace, high-speed rail, automobile and other fields, the use of high-strength or ultra-high-strength steel to achieve lightweight and improve safety has received more and more attention. At present, there are still some technical difficulties and challenges in the strong plasticity of high-strength and high-toughness steel. Chinese Patent 201911318107X discloses a production method for ultra-high plasticity twinning induced plasticity (TWIP) steel containing vanadium. The TWIP steel under this production method has good plasticity, and the elongation can reach up to 120%, but its yield strength is only about 200MPa, and the tensile strength is only about 500MPa, sacrificing a lot of strength. Chinese Patent 2021106016997 discloses a 1Mn6Ni austenitic steel with a tensile strength of up to 1500MPa. During the air cooling process after the steel plate is rolled, the austenite in the steel undergoes a martensitic phase transformation, accompanied by the precipitation of carbides. In the steel plate under this alloy composition and process, only carbides precipitate, and the precipitation strengthening mechanism cannot be effectively utilized to strengthen the steel plate. Chinese patent 202111202022 discloses a high-strength steel containing Ce and Ba, with a yield strength of 863MPa, a tensile strength of 1322MPa, and an elongation of 50.6%. The processing technology is low-temperature cold rolling, instantaneous annealing treatment and low-temperature tempering treatment in sequence. This process promotes the formation of twins and divides the grains, further reducing the mean free path of dislocation movement, thereby increasing the yield strength. However, the yield strength of this high-strength steel is very high, resulting in great deformation resistance and relatively poor processing performance. Further deepening the theoretical research and experimental exploration of the strength and plasticity of high-strength and high-toughness steels, developing new high-strength and high-toughness steel alloy systems and preparation processes, and expanding the application scope of the strength and plasticity of high-strength and high-toughness steels in the fields of automobiles, ships, machinery, etc. are currently important development directions in this field.
[0003] Chinese patent 201010173548.8 discloses a method of using the instantaneous impact effect of a pulsed magnetic field to promote the rapid movement of high-density dislocations in a material, inducing the formation of nano twins, and the composite material after treatment has the organizational characteristics of a nanoscale coherent interface. However, this method is only applicable to metals with relatively low stacking fault energy and prone to plastic deformation, such as Al, Mg or Ti.
[0004] In summary, the field is still seeking a method to obtain ultra-high strength and toughness steel that has high strength, high plasticity and is easy to process and form, while exploring processing and forming methods for forming high-strength and high-toughness steel. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides an ultra-high strength, high toughness steel and its preparation method and application. The steel of the present invention not only has ultra-high strength, high toughness and high plasticity, but also is easy to process and shape.
[0006] Magnetoplastic processing is a new type of processing technology, which applies a high-intensity magnetic field during the metal deformation process or uses a magnetic field to treat the metal before and after processing, so as to obtain metal materials with better mechanical properties and improve their processing performance. The present invention adds a specific content of vanadium (V) and niobium (Nb) to the steel, and combines it with a specific content of Mn, Cu, Al, Ni, and C, which has a higher stacking fault energy, promotes the transformation of the phase change induced plasticity effect (TRIP) to TWIP, and improves the strength and plasticity of the steel. The impact effect generated by low-frequency pulse current is used to improve the plasticity of metal materials and reduce deformation resistance. During the power-on process, the electromagnetic impact effect generated by the pulse current uses the free electrons inside the material to directional impact dislocations to achieve "depinning". And under the action of the electromagnetic field, radial pressure is applied to the blank, making the stamping deformation process easier, effectively reducing the quality requirements for the mold and the damage to the mold during the processing.
[0007] The preparation method provided by the present invention utilizes the principles of precipitation strengthening and grain refinement to make the prepared steel have good strength and plasticity. And by utilizing the low-temperature magneto-plastic processing technology, the high-strength and high-toughness steel with high yield strength has good processing performance, effectively reducing the quality requirements for the processing mold and the damage to the mold during the processing.
[0008] A first aspect of the present invention provides an ultra-high strength, high toughness steel.
[0009] Specifically, an ultra-high strength, high toughness steel, calculated by mass percentage, includes 18.00% to 24.50% manganese (Mn), 0.3% to 2.3% copper (Cu), 0.8% to 2.2% aluminum (Al), 0.5% to 2.2% niobium (Nb), 0.2% to 1.2% vanadium (V), 0.5% to 3.2% nickel (Ni), 0.07% to 0.8% carbon (C) and 63.6% to 79.63% Fe.
[0010] Preferably, the steel comprises, by mass percentage, 18.80% to 24.20% manganese (Mn), 0.5% to 2% copper (Cu), 1.0% to 2% aluminum (Al), 0.5% to 2% niobium (Nb), 0.2% to 1% vanadium (V), 0.5% to 3% nickel (Ni), 0.07% to 0.5% carbon (C) and 65.3% to 78.43% Fe.
[0011] Further preferably, the steel is composed, by mass percentage, of manganese (Mn) 18.80% to 24.20%, copper (Cu) 0.5% to 2%, aluminum (Al) 1.0% to 2%, niobium (Nb) 0.5% to 2%, vanadium (V) 0.2% to 1%, nickel (Ni) 0.5% to 3%, carbon (C) 0.07% to 0.5% and Fe as the remainder.
[0012] Preferably, the steel further includes inevitable impurities.
[0013] Preferably, the unavoidable impurities include phosphorus (P), sulfur (S), nitrogen (N), and oxygen (O).
[0014] Preferably, the unavoidable impurities, measured in mass percentage, include phosphorus (P) < 0.1%, sulfur (S) < 0.1%, nitrogen (N) < 25 ppm, and oxygen (O) < 25 ppm.
[0015] A second aspect of the present invention provides a method for preparing ultra-high strength and high toughness steel.
[0016] Specifically, a method for preparing ultra-high strength and high toughness steel comprises the following steps:
[0017] (1) Weighing each component, melting it, and continuously casting it to obtain a continuously cast slab;
[0018] (2) hot rolling the continuously cast slab obtained in step (1);
[0019] (3) After the treatment in step (2), warm rolling is performed;
[0020] (4) After the treatment in step (3), cooling and cold rolling are performed to obtain a cold-rolled slab;
[0021] (5) heating and keeping the cold-rolled slab warm by using an induction coil, and then quenching the slab to obtain a slab;
[0022] (6) pickling the slab obtained in step (5);
[0023] (7) Cooling the slab processed in step (6), and then placing it in an arc magnetic field formed by an electromagnet, passing an electric current to form a pulsed magnetic field to process the slab, thereby obtaining the ultra-high strength and high toughness steel.
[0024] Preferably, in step (1), refining is performed after smelting.
[0025] Preferably, in step (2), hot rolling is carried out at 1100-1300°C, and the final rolling temperature is 1000-1050°C.
[0026] Preferably, in step (3), after the treatment in step (2), the steel is further subjected to warm rolling treatment with a reduction of 30-60% per pass, a temperature of 500-700° C., and a time of 10-60 min.
[0027] Preferably, in step (4), the slab processed in step (3) is air-cooled to room temperature and then subjected to multiple cold rolling processes with a reduction of 60 to 80%.
[0028] Preferably, in step (5), the cold-rolled slab obtained in step (4) is rapidly heated to 500-700°C at 95-100°C / s using a high-frequency induction coil, kept at this temperature for 5-30 minutes, and then quenched to obtain a high-strength and high-toughness slab.
[0029] Preferably, in step (7), the slab treated in step (6) is cooled to below -190°C, for example -196°C, using liquid nitrogen.
[0030] Preferably, in step (7), the magnetic induction intensity of the pulsed magnetic field formed by passing current control is 10 to 50 T, and the magnetic field frequency is 0.1 to 5 Hz; further preferably, the magnetic induction intensity of the pulsed magnetic field formed by passing current control is 20 to 40 T, and the magnetic field frequency is 1 to 5 H.
[0031] Preferably, in step (7), a focusing magnetic core is installed in the electromagnet so that the arc magnetic field generated by the electromagnet can be more effectively concentrated in the processing area.
[0032] Step (7) effectively reduces the yield strength of the material through treatment with a pulsed magnetic field, making it easier to produce plastic deformation.
[0033] Preferably, the preparation method comprises the following steps:
[0034] (1) Weighing each component, melting the raw material with a purity of ≥99.9wt% in a melting device, refining after melting, and then continuously casting to produce a continuously cast slab with low center segregation, no cracks and high purity;
[0035] (2) hot rolling the continuously cast slab in step (1) at 1100-1300° C., with the final rolling temperature being 1000-1050° C.;
[0036] (3) subjecting the continuously cast slab in step (2) to a warm rolling treatment with a reduction of 30-60% per pass, a temperature of 500-700° C., and a time of 10-60 min;
[0037] (4) air cooling the slab in step (3) to room temperature, and then subjecting it to multiple cold rolling processes with a reduction of 60 to 80%;
[0038] (5) using a high-frequency induction coil to rapidly heat the cold-rolled slab in step (4) to 500-700° C. at 100° C. / s, keeping the temperature for 5-30 min, and then quenching to obtain a high-strength and high-toughness slab;
[0039] (6) pickling the high-strength and high-toughness slab in step (5) to remove the oxide layer on the surface of the slab;
[0040] (7) Use liquid nitrogen to cool the high-strength and high-toughness slab that has completed the surface treatment in step (6) to -196°C and place it on a workbench so that the slab is placed in an arc magnetic field formed by an electromagnet. Current is passed through the electromagnet to control the magnetic induction intensity of the pulsed magnetic field to be 10 to 50 T and the frequency of the magnetic field to be 0.1 to 5 Hz. A magnetic core is installed in the electromagnet so that the arc magnetic field generated by the electromagnet is more effectively concentrated in the processing area. The yield strength of the material is effectively reduced by the treatment of the pulsed magnetic field, making it easier to produce plastic deformation. Through repeated magnetoplasticity, low-temperature magnetoplastic stamping parts are obtained.
[0041] Preferably, in step (1), the smelting and refining process is carried out under an inert atmosphere of nitrogen or argon at 0.1 to 1 standard atmospheric pressure.
[0042] Preferably, in step (1), the smelting equipment is a medium frequency induction smelting furnace.
[0043] Preferably, in step (1), the temperature of the hot rolling treatment is 1200-1300°C.
[0044] Preferably, in step (3), the temperature of the warm rolling treatment is 600-700°C.
[0045] Preferably, in step (3), the temperature of the warm rolling treatment is 500-600°C.
[0046] Preferably, in step (3), the warm rolling treatment time is 15-25 minutes.
[0047] Preferably, in step (5), the temperature of the induction coil heating is 550-700°C, more preferably 550-600°C.
[0048] Preferably, in step (5), the induction coil heating time is 5 to 15 minutes, more preferably 5 to 10 minutes.
[0049] Preferably, in step (7), the pulse magnetic field intensity of the warm rolling treatment is 30T to 40T.
[0050] A third aspect of the present invention provides an application of ultra-high strength and high toughness steel.
[0051] The above-mentioned ultra-high strength and high toughness steel is used in aerospace, high-speed rail or automobile fields.
[0052] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0053] (1) The present invention adds specific contents of vanadium (V) and niobium (Nb) to the steel, and combines specific contents of Mn, Cu, Al, Ni, and C, so that the steel of the present invention has the characteristics of ultra-high strength, high toughness, and high plasticity.
[0054] (2) Use the impact effect generated by low-frequency pulse current to improve the plastic properties of metal materials and reduce deformation resistance. During the power-on process, the electromagnetic impact effect generated by the pulse current uses the free electrons inside the material to directional impact dislocations to achieve "depinning". And under the action of the electromagnetic field, radial pressure is applied to the blank, making the stamping deformation process easier, effectively reducing the quality requirements for the mold and the damage to the mold during the processing.
[0055] (3) The preparation method of the present invention first utilizes the precipitation strengthening mechanism to precipitate nano Ni-Al phases and produce high-density disordered copper-rich phases at the grain boundaries to strengthen high-strength steel. Secondly, the annealing, cold rolling and flash heat treatment processes control the grain size within a certain range, which not only refines the grains but also increases the nucleation sites of the precipitated phase, promotes the formation of the precipitated phase, and thus improves the yield strength and toughness. Finally, a low-temperature magnetoplastic process is used to effectively reduce the yield strength of the material, so that the high-yield strength high-strength and high-toughness steel has good processing properties, while greatly reducing the requirements for processing molds, reducing damage to the molds during processing, and extending the service life of the molds, so that the high-yield strength high-strength and high-toughness steel has good processing properties and is convenient for industrial processing. DETAILED DESCRIPTION
[0056] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0057] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0058] The model of the medium frequency induction furnace used in the embodiment of the present invention is SPZ-300.
[0059] In the embodiment of the present invention, pulse magnetic field stamping is adopted.
[0060] In the embodiment of the present invention, a SANS-CMT5105 electronic universal testing machine is used to perform stress-strain curve testing and obtain tensile strength.
[0061] Example 1: Preparation of ultra-high strength and high toughness steel
[0062] The invention discloses an ultra-high strength and high toughness steel having the following composition: in terms of mass percentage, manganese (Mn) 22%, copper (Cu) 1%, aluminum (Al) 1.5%, niobium (Nb) 1%, vanadium (V) 0.5%, nickel (Ni) 3%, carbon (C) 0.2%, phosphorus (P) < 0.1%, sulfur (S) < 0.1%, nitrogen (N) < 25ppm, oxygen (O) < 25ppm, and the balance is Fe.
[0063] A method for preparing ultra-high strength and high toughness steel comprises the following steps:
[0064] (1) In a nitrogen atmosphere at a standard atmospheric pressure, raw materials with a purity of ≥99.9wt% are melted in a melting device according to the above chemical composition and composition ratio, and after the melting is completed, they are refined and then continuously cast to produce a continuously cast slab with low center segregation, no cracks and high purity;
[0065] (2) hot rolling the continuously cast slab in step (1) at 1200° C., with the final rolling temperature being 1050° C.;
[0066] (3) the slab in step (2) is subjected to a warm rolling treatment with a reduction of 50% per pass, a temperature of 550° C., and a time of 20 min;
[0067] (4) air cooling the slab in step (3) to room temperature, and then subjecting it to multiple cold rolling processes with a reduction of 80%;
[0068] (5) heating the cold-rolled slab in step (4) to 550° C. by using a high-frequency induction coil, keeping the temperature for 5 min, and then quenching to obtain a high-strength and high-toughness slab;
[0069] (6) The high-strength and high-toughness slab in step (5) is pickled (0.1 mol / L hydrochloric acid) to remove the oxide layer on the surface of the slab;
[0070] (7) Use liquid nitrogen to cool the high-strength and high-toughness slab that has completed the pickling treatment in step (6) to minus 196°C and place it on a workbench, so that the slab is placed in an arc magnetic field formed by an electromagnet, and current is passed through the electromagnet to control the magnetic induction intensity of the formed pulse magnetic field to be 45T and the magnetic field frequency to be 0.5Hz. A magnetic core is installed in the electromagnet so that the arc magnetic field generated by the electromagnet can be more effectively concentrated in the processing area. Through the treatment of the pulse magnetic field, the yield strength of the material is effectively reduced, making it easier to produce plastic deformation. Through repeated magnetoplasticity, low-temperature magnetoplastic stamping parts are obtained, that is, steel is prepared.
[0071] With reference to GB / T 228.1-2010 "Tensile test of metallic materials Part 1: Room temperature test method", it is measured that the tensile strength of the steel prepared in this embodiment is 2036 MPa, the elongation is 41%, the yield strength is 1318 MPa, and it can be smoothly stamped by the above-mentioned magnetoplastic stamping method.
[0072] Example 2: Preparation of ultra-high strength and high toughness steel
[0073] The invention discloses an ultra-high strength and high toughness steel having the following composition: in terms of mass percentage, manganese (Mn) 18%, copper (Cu) 2.3%, aluminum (Al) 0.8%, niobium (Nb) 0.5%, vanadium (V) 1.2%, nickel (Ni) 0.5%, carbon (C) 0.8%, phosphorus (P) < 0.1%, sulfur (S) < 0.1%, nitrogen (N) < 25ppm, oxygen (O) < 25ppm, and the balance is Fe.
[0074] A method for preparing ultra-high strength and high toughness steel comprises the following steps:
[0075] (1) In a nitrogen atmosphere at a standard atmospheric pressure, raw materials with a purity of ≥99.9wt% are melted in a melting device according to the above chemical composition and composition ratio, and after the melting is completed, they are refined and then continuously cast to produce a continuously cast slab with low center segregation, no cracks and high purity;
[0076] (2) hot rolling the continuously cast slab in step (1) at 1200° C., with the final rolling temperature being 1050° C.;
[0077] (3) the slab in step (2) is subjected to a warm rolling treatment with a reduction of 50% per pass, a temperature of 550° C., and a time of 20 min;
[0078] (4) air cooling the slab in step (3) to room temperature, and then subjecting it to multiple cold rolling processes with a reduction of 80%;
[0079] (5) heating the cold-rolled slab in step (4) to 650° C. by using a high-frequency induction coil, keeping the temperature for 5 minutes, and then quenching to obtain a high-strength and high-toughness slab;
[0080] (6) The high-strength and high-toughness slab in step (5) is pickled (0.1 mol / L hydrochloric acid) to remove the oxide layer on the surface of the slab;
[0081] (7) Use liquid nitrogen to cool the high-strength and high-toughness slab that has been pickled in step (6) to -196°C and place it on a workbench so that the slab is placed in an arc magnetic field formed by an electromagnet. Current is passed through the electromagnet to control the magnetic induction intensity of the pulsed magnetic field to be 10T and the magnetic field frequency to be 0.1Hz. A magnet core is installed in the electromagnet so that the arc magnetic field generated by the electromagnet is more effectively concentrated in the processing area. Through the treatment of the pulsed magnetic field, the yield strength of the material is effectively reduced, making it easier to produce plastic deformation. Through repeated magneto-plasticity, a low-temperature magneto-plastic stamping part is obtained to obtain steel.
[0082] With reference to GB / T 228.1-2010 "Tensile test of metallic materials Part 1: Room temperature test method", it is measured that the tensile strength of the steel prepared in this embodiment is 1210 MPa, the elongation is 53%, the yield strength is 998 MPa, and it can be smoothly stamped by the above-mentioned magnetoplastic stamping method.
[0083] Example 3: Preparation of ultra-high strength and high toughness steel
[0084] The invention discloses an ultra-high strength and high toughness steel having the following composition: in terms of mass percentage, manganese (Mn) 24.5%, copper (Cu) 0.3%, aluminum (Al) 2.2%, niobium (Nb) 2.2%, vanadium (V) 0.2%, nickel (Ni) 3.2%, carbon (C) 0.07%, phosphorus (P) < 0.1%, sulfur (S) < 0.1%, nitrogen (N) < 25ppm, oxygen (O) < 25ppm, and the balance is Fe.
[0085] A method for preparing ultra-high strength and high toughness steel comprises the following steps:
[0086] (1) In a nitrogen atmosphere at a standard atmospheric pressure, raw materials with a purity of ≥99.9wt% are melted in a melting device according to the above chemical composition and composition ratio, and after the melting is completed, they are refined and then continuously cast to produce a continuously cast slab with low center segregation, no cracks and high purity;
[0087] (2) hot rolling the continuously cast slab in step (1) at 1200° C., with the final rolling temperature being 1050° C.;
[0088] (3) the slab in step (2) is subjected to a warm rolling treatment with a reduction of 50% per pass, a temperature of 650° C., and a time of 20 min;
[0089] (4) air cooling the slab in step (3) to room temperature, and then subjecting it to multiple cold rolling processes with a reduction of 80%;
[0090] (5) heating the cold-rolled slab in step (4) to 650° C. by using a high-frequency induction coil, keeping the temperature for 5 minutes, and then quenching to obtain a high-strength and high-toughness slab;
[0091] (6) The high-strength and high-toughness slab in step (5) is pickled (0.1 mol / L hydrochloric acid) to remove the oxide layer on the surface of the slab;
[0092] (7) Use liquid nitrogen to cool the high-strength and high-toughness slab that has completed the pickling treatment in step (6) to -196°C and place it on a workbench, so that the slab is placed in an arc magnetic field formed by an electromagnet, and current is passed through the electromagnet to control the magnetic induction intensity of the formed pulse magnetic field to be 50T and the magnetic field frequency to be 5Hz. A magnetic core is installed in the electromagnet so that the arc magnetic field generated by the electromagnet can be more effectively concentrated in the processing area. Through the treatment of the pulse magnetic field, the yield strength of the material is effectively reduced, making it easier to produce plastic deformation. Through repeated magnetoplasticity, low-temperature magnetoplastic stamping parts are obtained to obtain steel.
[0093] With reference to GB / T 228.1-2010 "Tensile test of metallic materials Part 1: Room temperature test method", it is measured that the tensile strength of the steel prepared in this embodiment is 1894 MPa, the elongation is 42%, the yield strength is 1624 MPa, and it can be smoothly stamped by the above-mentioned magnetoplastic stamping method.
[0094] Comparative Example 1
[0095] Compared with Example 1, the only difference of Comparative Example 1 is that the niobium (Nb) content is 0.4%, and the rest of the composition and process are the same as those of Example 1.
[0096] The steel prepared in this comparative example has a tensile strength of 1126 MPa, an elongation of 49%, and a yield strength of 963 MPa.
[0097] Comparative Example 2
[0098] Compared with Example 1, the only difference of Comparative Example 2 is that the vanadium (V) content is 0.1%, and the rest of the composition and process are the same as those of Example 1.
[0099] The steel prepared in this comparative example has a tensile strength of 1040 MPa, an elongation of 31%, and a yield strength of 909 MPa.
Claims
1. A type of steel, It is characterized in that The invention is composed of the following components in terms of mass percentage: Mn 18.00% to 24.50%, Cu 0.3% to 2.3%, Al 0.8% to 2.2%, Nb 0.5% to 2.2%, V 0.2% to 1.2%, Ni 0.5% to 3.2%, C 0.07% to 0.8% and Fe 63.6% to 79.63%, and inevitable impurities, wherein the inevitable impurities include P, S, N and O; The method for preparing the steel comprises the following steps: (1) Weighing each component, melting it, and continuously casting it to obtain a continuously cast slab; (2) hot rolling the continuously cast slab obtained in step (1); (3) After the treatment in step (2), warm rolling is performed; (4) After the treatment in step (3), cooling and cold rolling are performed to obtain a cold-rolled slab; (5) heating and keeping the cold-rolled slab warm by using an induction coil, and then quenching the slab to obtain a slab; (6) pickling the slab obtained in step (5); (7) cooling the slab processed in step (6), and then placing it in an arc magnetic field formed by an electromagnet, passing an electric current to form a pulsed magnetic field to process the slab, thereby obtaining the steel; In step (2), hot rolling is carried out at 1100-1300° C., and the final rolling temperature is 1000-1050° C.; In step (3), after the treatment in step (2), the steel is further subjected to warm rolling with a reduction of 30-60% per pass, a temperature of 500-700° C., and a time of 10-60 min; In step (5), the cold-rolled slab obtained in step (4) is rapidly heated to 500-700° C. at 95-100° C. / s by a high-frequency induction coil, kept at this temperature for 5-30 minutes, and then quenched to obtain a slab; In step (7), the slab treated in step (6) is cooled to below -190°C using liquid nitrogen, and a pulsed magnetic field is passed through the slab to control the magnetic induction intensity to be 10 to 50 T and the magnetic field frequency to be 0.1 to 5 Hz.
2. The steel according to claim 1, It is characterized in that In terms of mass percentage, it is composed of the following components: Mn 18.80% to 24.20%, Cu 0.5% to 2%, Al 1.0% to 2%, Nb 0.5% to 2%, V0.2% to 1%, Ni0.5% to 3%, C 0.07%-0.5% and Fe 65.3%-78.43%, and inevitable impurities, wherein the inevitable impurities include P, S, N, and O.
3. The steel according to claim 1, It is characterized in that The unavoidable impurities, in terms of mass percentage, include P < 0.1%, S < 0.1%, N < 25 ppm, and O < 25 ppm.
4. The method for preparing the steel according to any one of claims 1 to 3, It is characterized in that The following steps are involved: (1) Weighing each component, melting it, and continuously casting it to obtain a continuously cast slab; (2) hot rolling the continuously cast slab obtained in step (1); (3) After the treatment in step (2), warm rolling is performed; (4) After the treatment in step (3), cooling and cold rolling are performed to obtain a cold-rolled slab; (5) heating and keeping the cold-rolled slab warm by using an induction coil, and then quenching the slab to obtain a slab; (6) pickling the slab obtained in step (5); (7) cooling the slab processed in step (6), and then placing it in an arc magnetic field formed by an electromagnet, passing an electric current to form a pulsed magnetic field to process the slab, thereby obtaining the steel; In step (2), hot rolling is carried out at 1100-1300° C., and the final rolling temperature is 1000-1050° C.; In step (3), after the treatment in step (2), the steel is further subjected to warm rolling with a reduction of 30-60% per pass, a temperature of 500-700° C., and a time of 10-60 min; In step (5), the cold-rolled slab obtained in step (4) is rapidly heated to 500-700° C. at 95-100° C. / s by a high-frequency induction coil, kept at this temperature for 5-30 minutes, and then quenched to obtain a slab; In step (7), the slab treated in step (6) is cooled to below -190°C using liquid nitrogen, and a pulsed magnetic field is passed through the slab to control the magnetic induction intensity to be 10 to 50 T and the magnetic field frequency to be 0.1 to 5 Hz.
5. The preparation method according to claim 4, It is characterized in that In step (4), the slab processed in step (3) is air-cooled to room temperature and then subjected to multiple cold rolling processes with a reduction of 60 to 80%.