A hollow, internally mounted square steel tube concrete component

By using materials such as silane-modified steel fiber and epoxy resin emulsion in hollow built-in square steel tube concrete components, the challenge of improving the mechanical properties of the components is solved, achieving higher fire resistance and structural strength, reducing self-weight and protective measures need.

CN118148295BActive Publication Date: 2024-10-01CENTRAL SOUTH UNIVERSITY OF FORESTRY AND TECHNOLOGY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410281585.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-12
Publication Date
2024-10-01
Estimated Expiration
2044-03-12

AI Technical Summary

Technical Problem

There is room for improvement in the mechanical properties of existing hollow built-in square steel tube concrete members, especially in buildings that bear greater loads and higher heights. How to further improve their seismic performance and structural strength has become a research hotspot.

Method used

It uses square steel pipes, steel cages and special concrete raw materials, including silane modified steel fibers, water-based polyurethane emulsions, epoxy resin emulsions and organic alcohol amines, to improve the bonding properties of steel fibers and cement, the compactness and microscopic properties of concrete. porous structure to enhance the mechanical properties of concrete.

Benefits of technology

It effectively improves the fire resistance of components, avoids corrosion and slippage of steel pipes, enhances the mechanical strength and structural stability of concrete, reduces the amount of concrete and the need for fire and rust prevention measures, and improves the overall structural strength of the building.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118148295B_ABST
    Figure CN118148295B_ABST
Patent Text Reader

Abstract

The invention relates to the field of building construction structural components, in particular to a hollow built-in square steel tube concrete component, comprising a square steel tube, a steel cage and concrete; the square steel tube comprises a tube body and steel bolts arranged around the tube body; the concrete is made of the following raw materials in parts by weight: 80-100 parts of cement, 10-20 parts of silane-modified steel fiber, 100-120 parts of quartz sand, 20-30 parts of fly ash, 5-10 parts of water-based polyurethane emulsion, 10-20 parts of epoxy resin emulsion, 1-5 parts of styrene-acrylic emulsion, 0.5-1 parts of polycarboxylic acid water reducer, 0.1-1 parts of organic alcohol amine, 0.1-1 parts of defoamer and 20-40 parts of water. The concrete mortar prepared by the invention has good mechanical strength, and as a preparation material of a concrete component, it plays a key role in further improving its structural strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building construction structural components, in particular to a hollow built-in square steel tube concrete component. Background Art

[0002] With the continuous development of society, buildings are developing towards larger spans and higher heights. The load borne by the load-bearing components increases, and the self-weight also increases accordingly. This puts higher requirements on the component form of the building. The hollow built-in square steel tube concrete formed by adding steel sections inside the reinforced concrete can reduce the self-weight of the concrete components and improve the seismic performance of the concrete components. The lateral constraint of concrete on the steel also ensures that the mechanical properties of the steel are fully exerted and will not be withdrawn from work prematurely due to instability. However, how to further improve the mechanical properties of steel tube concrete components has become a current research hotspot. Summary of the invention

[0003] Purpose of the invention: In view of the above technical problems, the present invention proposes a hollow built-in square steel tube concrete component.

[0004] The technical solutions adopted are as follows:

[0005] A hollow built-in square steel tube concrete component, comprising a square steel tube, a steel cage and concrete;

[0006] The square steel pipe comprises a pipe body and steel bolts arranged around the pipe body;

[0007] The concrete is made of the following raw materials in parts by weight:

[0008] 80-100 parts of cement, 10-20 parts of silane modified steel fiber, 100-120 parts of quartz sand, 20-30 parts of fly ash, 5-10 parts of water-based polyurethane emulsion, 10-20 parts of epoxy resin emulsion, 1-5 parts of styrene acrylic emulsion, 0.5-1 parts of polycarboxylic acid water reducer, 0.1-1 parts of organic alcohol amine, 0.1-1 parts of defoaming agent, and 20-40 parts of water.

[0009] Furthermore, the preparation method of the silane-modified steel fiber is as follows:

[0010] The steel fiber is immersed in a sodium hydroxide solution for more than 1 hour, taken out and washed with water, then added into a silane hydrolyzate solution and stirred for modification treatment for more than 1 hour, taken out and placed in an oven at a temperature above 100° C. for heat treatment for 1-10 hours.

[0011] Furthermore, the configuration method of the silane hydrolyzate is as follows:

[0012] Mix methanol and water in proportion, add silane and stir for 10-60 minutes, adjust the pH to 3-5 with acetic acid, and seal and hydrolyze for more than 24 hours.

[0013] Furthermore, the silane is KH-560.

[0014] Furthermore, the preparation method of the epoxy resin emulsion is as follows:

[0015] The epoxy resin E-44 is dissolved in a mixed solvent consisting of ethanol and ethylene glycol monomethyl ether, and the temperature is raised to 75-85°C under nitrogen protection, and an acetone solution containing a free radical initiator is added dropwise. After the addition is completed, the temperature is raised to 100-110°C with stirring, and a mixed monomer consisting of 2-methyl-2-acrylamide-propanesulfonic acid, acrylic acid and methyl acrylate is added. After continuing the reaction for 3-6 hours, the solvent is evaporated off, an emulsifier is added, and the stirring speed is adjusted to 1500-2500r / min. After adding water and strong shear stirring, the epoxy resin emulsion can be obtained.

[0016] Furthermore, the weight ratio of the 2-methyl-2-acrylamide-propanesulfonic acid, acrylic acid and methyl acrylate is 1:0.3-0.5:0.1-0.2.

[0017] Furthermore, the weight ratio of the epoxy resin E-44 to the mixed monomer is 1:0.8-1.

[0018] Furthermore, the emulsifier is composed of OP-10 and sodium dodecyl sulfate in a weight ratio of 1-5:1-5.

[0019] Furthermore, the organic alcohol amine is any one or more combinations of monoethanolamine, diethanolamine and triethanolamine.

[0020] Furthermore, the defoamer is composed of an organosilicon defoamer and a polyether defoamer in a weight ratio of 1-5:1-5.

[0021] Beneficial effects of the present invention:

[0022] The present invention provides a hollow built-in square steel tube concrete component. Since the built-in square steel tube is wrapped by concrete, air and moisture are isolated, which plays a good protective role on the square steel tube, not only effectively avoiding the corrosion of the square steel tube, but also significantly improving the fire resistance of the structure, eliminating the need for fire prevention and rust prevention measures for the square steel tube, and also saving the amount of concrete. The tube body with steel bolts around it can improve the bonding performance of the square steel tube and concrete, and avoid slippage under strong external force.

[0023] The active groups on the surface of silane-modified steel fibers can establish chemical bonds with cement, which enhances the bonding performance of the interface between steel fibers and cement matrix, and improves the mechanical properties of concrete. Waterborne polyurethane emulsions, epoxy resin emulsions and styrene acrylic emulsions improve the workability of concrete, making it easier to compact and smaller in pores under vibration. After the polymer emulsion loses water and forms a film, it helps to block and fill the macropores and interconnected pores in the concrete, improves the microscopic pore structure of the concrete, and helps to improve the mechanical strength of the concrete. The self-made epoxy resin emulsion introduces the polar group sulfonic acid group, which has better water solubility. The side chains containing sulfonic acid groups can provide bridging effects to increase the interaction between cement particles, improve the working performance of concrete, and improve the mechanical strength of concrete.

[0024] Organic alcohol amines can be used as curing agents for epoxy resin emulsions, and can also increase the strength of concrete, improve the durability of concrete, and prevent cracking and falling off of concrete. The combination of silicone defoamers and polyether defoamers can eliminate the bubbles introduced by polymer emulsions in concrete mortar, effectively improving the mechanical properties of concrete and reducing its shrinkage rate.

[0025] The concrete mortar prepared by the present invention has good mechanical strength and plays a key role as a preparation material for concrete components in further improving their structural strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a schematic structural diagram of a concrete component prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0027] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.

[0028] Cement: P.O42.5R ordinary Portland cement, Conch;

[0029] Silane modified steel fiber: homemade;

[0030] Quartz sand: fineness modulus is 2.83; Shijiazhuang Shiye Mineral Products Co., Ltd.;

[0031] Fly ash: Shijiazhuang Bennuo Mineral Products Co., Ltd.;

[0032] Water-based polyurethane emulsion: TK2109, brand: Taikang;

[0033] Epoxy resin emulsion: homemade;

[0034] Styrene acrylic emulsion: Shandong Xinrunjin Chemical Co., Ltd.;

[0035] Polycarboxylate water reducer: Shandong Huibang New Material Technology Co., Ltd.;

[0036] Triethanolamine: Shandong Baihua Chemical Co., Ltd.;

[0037] Silicone defoamer: THIX-278, Yantai Hengxin Chemical Technology Co., Ltd.;

[0038] Polyether defoamer: THIX-288, Yantai Hengxin Chemical Technology Co., Ltd.;

[0039] Water: tap water.

[0040] Embodiment 1:

[0041] A hollow built-in square steel tube concrete component, comprising a square steel tube 1, a steel cage 2 and concrete 3;

[0042] The square steel pipe 1 comprises a pipe body 101 and steel bolts 102 arranged around the pipe body;

[0043] Concrete 4 is made of the following raw materials in parts by weight:

[0044] 90 parts of cement, 15 parts of silane modified steel fiber, 100 parts of quartz sand, 25 parts of fly ash, 5 parts of water-based polyurethane emulsion, 15 parts of epoxy resin emulsion, 5 parts of styrene acrylic emulsion, 0.5 parts of polycarboxylic acid water reducer, 0.5 parts of triethanolamine, 0.25 parts of silicone defoamer, 0.25 parts of polyether defoamer, and 35 parts of water.

[0045] Wherein, the preparation method of silane modified steel fiber is as follows:

[0046] 100 ml of methanol and 600 ml of water were mixed in proportion, 100 ml of KH-560 was added and stirred for 30 min, the pH was adjusted to 4 with acetic acid, and the silane hydrolyzate was obtained by sealed hydrolysis for 36 h. 100 g of steel fiber (diameter 0.18-0.22 mm, length 12-14 mm, tensile strength ≥ 2850 MPa) was immersed in a 20% sodium hydroxide solution for 2 h, the steel fiber was taken out and washed with water, and then added to the above silane hydrolyzate, and the modified treatment was stirred at room temperature for 2 h. The steel fiber was taken out and drained, and then placed in an oven at a temperature of 110 ° C for heat treatment for 5 h.

[0047] The preparation method of epoxy resin emulsion is as follows:

[0048] 540g of epoxy resin E-44 was added to a reaction kettle with a condenser, dissolved with 5000ml of a mixed solvent consisting of ethanol and ethylene glycol monomethyl ether (1:1, v / v), heated to 80°C under nitrogen protection, and 100ml of an acetone solution containing 15g of a free radical initiator BPO was added dropwise. After the addition was completed, the mixture was stirred and heated to 105°C. A mixed monomer consisting of 300g of 2-methyl-2-acrylamide-propanesulfonic acid, 150g of acrylic acid and 30g of methyl acrylate was added. After the reaction was continued for 5h, the solvent was evaporated, and 150g of an emulsifier consisting of OP-10 and sodium dodecyl sulfate in a weight ratio of 1:1 was added, and the stirring speed was adjusted to 2000r / min. An epoxy resin emulsion with a solid content of 50% was obtained after adding an appropriate amount of water and strong shear stirring.

[0049] The preparation method of the above concrete component is as follows:

[0050] Add cement, silane-modified steel fiber, quartz sand and fly ash into a mixer, dry mix for 5 minutes, add half of the water and stir for 4 minutes, then add the other half of the water, water-based polyurethane emulsion, epoxy resin emulsion, styrene-acrylic emulsion, polycarboxylic acid water reducer, silicone defoamer and polyether defoamer, stir for 5 minutes, then add triethanolamine and stir for another 5 minutes to obtain concrete mortar, pour the concrete mortar into a mold, in which a square steel pipe and a steel cage 2 are placed in advance, the concrete mortar is poured into the space between the inner wall of the mold and the outer wall of the square steel pipe, and the steel cage 2 is wrapped, the mold is fixed, and vibrated on a vibration table for about 1 minute at a vibration frequency of 50 Hz. After initial setting, the mold is removed and the mold is moved into a curing box with a temperature of (23±1)°C and a relative humidity of> 90% for curing for 28 days.

[0051] Embodiment 2:

[0052] A hollow built-in square steel tube concrete component, comprising a square steel tube, a steel cage and concrete;

[0053] The square steel pipe includes a pipe body and steel bolts arranged around the pipe body;

[0054] Concrete is made from the following raw materials, in parts by weight:

[0055] 100 parts of cement, 20 parts of silane modified steel fiber, 120 parts of quartz sand, 30 parts of fly ash, 10 parts of water-based polyurethane emulsion, 15 parts of epoxy resin emulsion, 5 parts of styrene acrylic emulsion, 1 part of polycarboxylic acid water reducer, 1 part of triethanolamine, 0.5 parts of silicone defoamer, 0.5 parts of polyether defoamer, and 40 parts of water.

[0056] The preparation method of silane-modified steel fiber, epoxy resin emulsion and concrete component is the same as that in Example 1.

[0057] Embodiment 3:

[0058] A hollow built-in square steel tube concrete component, comprising a square steel tube, a steel cage and concrete;

[0059] The square steel pipe includes a pipe body and steel bolts arranged around the pipe body;

[0060] Concrete is made from the following raw materials, in parts by weight:

[0061] 80 parts of cement, 10 parts of silane modified steel fiber, 100 parts of quartz sand, 20 parts of fly ash, 5 parts of water-based polyurethane emulsion, 10 parts of epoxy resin emulsion, 1 part of styrene acrylic emulsion, 0.5 parts of polycarboxylic acid water reducer, 0.1 parts of triethanolamine, 0.1 parts of silicone defoamer, 0.1 parts of polyether defoamer, and 30 parts of water.

[0062] The preparation method of silane-modified steel fiber, epoxy resin emulsion and concrete component is the same as that in Example 1.

[0063] Comparative Example 1:

[0064] It is basically the same as Example 1, except that the steel fiber is not modified by silane.

[0065] Comparative Example 2:

[0066] The method is basically the same as Example 1, except that no aqueous polyurethane emulsion is added.

[0067] Comparative Example 3:

[0068] The method is substantially the same as Example 1, except that no styrene acrylic emulsion is added.

[0069] Comparative Example 4:

[0070] The method is basically the same as Example 1, except that no epoxy resin emulsion is added.

[0071] Comparative Example 5:

[0072] The method is substantially the same as Example 1, except that a commercially available epoxy resin emulsion (brand: DOW Chemical, model: DER WB3002) is used instead of the homemade epoxy resin emulsion.

[0073] Comparative Example 6:

[0074] The method is basically the same as Example 1, except that no silicone defoaming agent is added.

[0075] Comparative Example 7:

[0076] The method is basically the same as Example 1, except that no polyether defoamer is added.

[0077] Comparative Example 8:

[0078] The method is basically the same as Example 1, except that a polyether-modified silicone defoamer (THIX-299, Yantai Hengxin Chemical Technology Co., Ltd.) is used instead of the silicone defoamer and the polyether defoamer.

[0079] Performance Test:

[0080] The concrete mortars prepared in Examples 1-3 and Comparative Examples 1-8 were prepared into test pieces and performance tests were performed;

[0081] The flexural strength and compressive strength of the sample were measured with reference to the specification "Test Method for Strength of Cement Mortar (ISO Method)" (GB / T 17671-1999). The test results are shown in Table 1:

[0082] Table 1:

[0083]

[0084] It can be seen from Table 1 above that the concrete mortar prepared by the present invention has good mechanical strength, and as a preparation material for concrete components, it plays a key role in further improving their structural strength.

[0085] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A hollow built-in square steel tube concrete component, characterized in that: Includes square steel pipes, steel cages and concrete; The square steel pipe comprises a pipe body and steel bolts arranged around the pipe body; The concrete is made of the following raw materials in parts by weight: 80-100 parts of cement, 10-20 parts of silane-modified steel fiber, 100-120 parts of quartz sand, 20-30 parts of fly ash, 5-10 parts of waterborne polyurethane emulsion, 10-20 parts of epoxy resin emulsion, 1-5 parts of styrene-acrylic emulsion, 0.5-1 parts of polycarboxylic acid water reducer, 0.1-1 parts of organic alcohol amine, 0.1-1 parts of defoaming agent, and 20-40 parts of water; The preparation method of the silane-modified steel fiber is as follows: The steel fiber is immersed in a sodium hydroxide solution for more than 1 hour, taken out and washed with water, then added into a silane hydrolyzate solution and stirred for modification for more than 1 hour, taken out and placed in an oven at a temperature of more than 100°C for heat treatment for 1-10 hours; The configuration method of the silane hydrolyzate is as follows: Mix methanol and water in proportion, add silane and stir for 10-60 minutes, adjust the pH to 3-5 with acetic acid, and seal and hydrolyze for more than 24 hours; The silane is KH-560; The preparation method of the epoxy resin emulsion is as follows: The epoxy resin E-44 is dissolved in a mixed solvent consisting of ethanol and ethylene glycol monomethyl ether, and the temperature is raised to 75-85°C under nitrogen protection, and an acetone solution containing a free radical initiator is added dropwise. After the addition is completed, the temperature is raised to 100-110°C with stirring, and a mixed monomer consisting of 2-methyl-2-acrylamide-propanesulfonic acid, acrylic acid and methyl acrylate is added. After continuing the reaction for 3-6 hours, the solvent is evaporated off, an emulsifier is added, and the stirring speed is adjusted to 1500-2500r / min. After adding water and strong shear stirring, the epoxy resin emulsion can be obtained.

2. The hollow inner square steel tube concrete member according to claim 1, characterized in that: The weight ratio of the 2-methyl-2-acrylamide-propanesulfonic acid, acrylic acid and methyl acrylate is 1:0.3-0.5:0.1-0.

2.

3. The hollow inner square steel tube concrete member according to claim 1, characterized in that: The weight ratio of the epoxy resin E-44 to the mixed monomer is 1:0.8-1.

4. The hollow inner square steel tube concrete member according to claim 1, characterized in that: The emulsifier is composed of OP-10 and sodium dodecyl sulfate in a weight ratio of 1-5:1-5.

5. The hollow inner square steel tube concrete member according to claim 1, characterized in that: The organic alcohol amine is any one or more combinations of monoethanolamine, diethanolamine and triethanolamine.

6. The hollow inner square steel tube concrete member according to claim 1, characterized in that: The defoamer is composed of an organic silicon defoamer and a polyether defoamer in a weight ratio of 1-5:1-5.