Silicon-carbon negative electrode material for lithium-ion battery and preparation method thereof
The uneven deposition of silicon carbon anode materials in lithium-ion batteries was solved by screening porous carbon matrix through low-field nuclear magnetic resonance and vapor deposition of nanosilicon and carbon coating on it, which significantly improved the electrochemical performance and low-temperature rate performance .
Patent Information
- Application Number
- CN202410170304.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-02-06
AI Technical Summary
The application of silicon-carbon anode materials in lithium-ion batteries is affected by the problems of agglomeration and low conductivity caused by the uneven deposition of nano-silicon in porous carbon, which affects the electrochemical performance.
By characterizing the low-field nuclear magnetic resonance, the screening carbon matrix with controllable structure, rich pores and uniform pore size distribution, the nanosilicon was vapor-deposited and the carbon layer was coated on the outer surface to prepare a silicon-carbon negative electrode material with excellent electrochemical properties.
It has achieved high-efficiency electrochemical performance of lithium-ion batteries, especially in terms of 0.8V first-effect and low-temperature rate performance, which has performed more than 80%.
Smart Images

Figure CN118156450B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of negative electrode materials for lithium ion batteries, and in particular to a silicon-carbon negative electrode material for lithium ion batteries and a preparation method thereof. Background Art
[0002] Silicon (Si) is considered to be a high-capacity anode material for next-generation lithium-ion batteries due to its high theoretical specific capacity (4200 mAh / g). However, the large volume change of silicon anode (>300%) and its low intrinsic conductivity lead to the + The limited diffusion capacity seriously hinders the commercial application of silicon negative electrodes.
[0003] Nano-sizing of silicon can effectively alleviate the above-mentioned problems. Currently, silicon-carbon negative electrode materials prepared by CVD method are widely studied. They mainly use silane as raw material to deposit nano-silicon on porous carbon matrix by CVD, and then perform carbon coating, which alleviates the expansion problem of nano-silicon and improves the conductivity of the material. However, the uniformity of nano-silicon deposition in porous carbon mainly depends on whether the porous carbon matrix has controllable structure, rich pores and uniform pore size distribution. Porous carbon has the characteristics of high specific surface area and complex pore structure, which brings great uncertainty to the application of porous carbon. Uneven deposition of nano-silicon will lead to the agglomeration of nano-silicon and deposition on the outer surface of porous carbon, which seriously affects the performance of silicon-carbon negative electrode materials and further affects the electrochemical performance of lithium-ion batteries. Summary of the invention
[0004] In order to obtain a lithium-ion battery with better electrochemical performance, a silicon-carbon negative electrode material for a lithium-ion battery and a preparation method thereof are provided. The present invention characterizes the porous carbon matrix by low-field nuclear magnetic resonance, screens out a porous carbon matrix with controllable structure, rich pores and uniform pore size distribution, and applies the silicon-carbon negative electrode prepared by the method to a lithium battery, so that the battery has better electrochemical performance.
[0005] In order to achieve the above objectives, the present invention is implemented by the following technical solutions:
[0006] A silicon-carbon negative electrode material for a lithium-ion battery, wherein the structure of the silicon-carbon negative electrode material is based on a porous carbon matrix as a core, a vapor-deposited nano-silicon material is present in the porous carbon matrix, and a carbon coating layer is present on the outer surface of the porous carbon matrix;
[0007] The pore size distribution of the porous carbon matrix measured by low-field nuclear magnetic resonance satisfies one of the following conditions:
[0008] ①0.2nm-7nm has a bimodal distribution;
[0009] ② It has a bimodal distribution below 1nm, one peak below 0.1nm, and one peak between 0.1nm-1nm.
[0010] Furthermore, the silicon-carbon negative electrode material is calculated based on 100% by weight: the vapor-deposited nano-silicon material accounts for 30wt%-70wt%, the carbon coating layer accounts for 0wt%-5wt%, and the remainder is the porous carbon matrix.
[0011] Preferably, the silicon-carbon negative electrode material is calculated based on 100% by weight: the vapor-deposited nano-silicon material accounts for 50wt%-70wt%, the carbon coating layer accounts for 1wt%-3wt%, and the remainder is the porous carbon matrix.
[0012] Furthermore, the total pore volume of the porous carbon matrix is 0.5 cm 3 / g or more, with a specific surface area of 800m 2 / g or more;
[0013] The particle size of the porous carbon matrix is between 0.1 microns and 40 microns, wherein the minimum particle size Dmin is between 0.1 microns and 2 microns, the average particle size D50 is between 5 microns and 10 microns, and the maximum particle size D100 is between 15 microns and 30 microns;
[0014] The compaction density of the porous carbon matrix is 0.8 cm 3 / g-1.4cm 3 / g;
[0015] The oxygen content of the porous carbon matrix is between 0.5wt% and 3.0wt%.
[0016] Another aspect of the present invention provides a method for preparing the silicon-carbon negative electrode material for the above-mentioned lithium ion battery, comprising the following steps:
[0017] Porous carbon is added to a reaction container as a deposition substrate, protective gas is introduced to replace the air in the reaction container, and then the temperature is raised to a reaction temperature of 400-650° C., and silane gas is introduced at a flow rate of 10 L / min-40 L / min to vapor-deposit nano-silicon material in the porous carbon matrix for 5-20 hours. After the deposition is completed, a deposited silicon porous carbon material is obtained;
[0018] The reaction temperature is maintained, and then a gaseous carbon source is introduced at 1-20 L / min to carbon-coat the deposited silicon porous carbon material. The carbon coating time is 1-5 hours. After the reaction is completed, a silicon-carbon negative electrode material is obtained.
[0019] Furthermore, the protective gas is nitrogen or argon, and the flow rate of the protective gas is 6L / min-24L / min; the heating rate is 1-10°C / min.
[0020] Furthermore, the silane gas is selected from one or more of dichlorosilane, monosilane, disilane, and trisilane; and the gaseous carbon source is selected from one or more of acetylene, methane, ethylene, and propylene.
[0021] Beneficial technical effects:
[0022] The structure of the silicon-carbon negative electrode material of the present invention is based on a porous carbon matrix as the core, with vapor-deposited nano-silicon material in the porous carbon matrix and a carbon coating layer on the outer surface of the porous carbon matrix; the nano-silicon material is formed by vapor deposition as an electrochemical material; the carbon coating layer on the surface is used to improve the conductivity of the material; the present invention characterizes and screens the porous carbon matrix by low-field nuclear magnetic resonance method to find out that the pore size distribution meets one of the following conditions: ① 0.2nm-7nm has a bimodal distribution; ② below 1nm has a bimodal distribution, and there is one peak below 0.1nm and one peak between 0.1nm-1nm. The prepared silicon-carbon negative electrode material has a 0.8V first efficiency of more than 80% for lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is the nitrogen adsorption isotherm curve corresponding to porous carbon samples V, VI, IX, and X;
[0024] Figure 2 The low-field NMR inversion curves and T2 relaxation spectra of porous carbon samples V, VI, IX, and X;
[0025] Figure 3 This is a comparison chart of the pore size distribution curves of porous carbon sample Ⅶ measured by gas adsorption method and low-field nuclear magnetic resonance method;
[0026] Figure 4 This is the pore size distribution diagram of porous carbon sample Ⅰ measured by low-field nuclear magnetic resonance;
[0027] Figure 5 This is the pore size distribution diagram of porous carbon sample II measured by low-field nuclear magnetic resonance;
[0028] Figure 6 This is the pore size distribution diagram of porous carbon sample III measured by low-field nuclear magnetic resonance;
[0029] Figure 7 This is the pore size distribution diagram of porous carbon sample IV measured by low-field nuclear magnetic resonance;
[0030] Figure 8 This is the pore size distribution diagram of porous carbon sample V measured by low-field nuclear magnetic resonance;
[0031] Fig. 9 This is the pore size distribution diagram of porous carbon sample VI measured by low-field nuclear magnetic resonance;
[0032] Fig.10This is the pore size distribution diagram of porous carbon sample Ⅶ measured by low-field nuclear magnetic resonance;
[0033] Fig.11 This is the pore size distribution diagram of porous carbon sample VIII measured by low-field nuclear magnetic resonance;
[0034] Fig.12 This is the pore size distribution diagram of porous carbon sample IX measured by low-field nuclear magnetic resonance;
[0035] Fig.13 is the pore size distribution diagram of porous carbon sample X measured by low-field nuclear magnetic resonance;
[0036] Fig.14 This is a low-temperature rate performance diagram of lithium-ion batteries made of the silicon-carbon negative electrode materials prepared in Example 1, Example 4, and Example 5 at -20°C. DETAILED DESCRIPTION
[0037] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention are within the scope of protection of the present invention.
[0038] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.
[0039] The experimental methods in the following examples without specifying specific conditions are usually measured in accordance with national standards; if there is no corresponding national standard, they are carried out in accordance with general standard requirements or general methods.
[0040] Test Example 1
[0041] At present, the commonly used method to characterize the pore structure of porous carbon is the gas adsorption method, which uses small molecular gases such as nitrogen, carbon dioxide, and helium as adsorbents to measure the adsorption isotherm curve of the sample (such as Figure 1is the nitrogen adsorption isotherm), and the specific surface area, pore volume and pore size distribution are obtained through simulation calculations of various models such as BET, BJH, and DFT. In recent years, with the gradual improvement of various model algorithms, this method has played an important role in testing the pore structure information of micro-mesoporous (0-50nm) samples. However, this method still has some defects: in order to improve the accuracy of the test, a long test time is often required; on the other hand, the only pore structure information intuitively obtained by the gas adsorption method is the adsorption isotherm, while the pore size distribution obtained from the simulation calculation of various models presents an ideal state. For example, the BET theory ignores the lateral interactions between adsorbed molecules and assumes that all adsorption sites are energy equivalent. The filling of the adsorbate in the pore is affected by the pore shape and the surface properties of the pore wall, resulting in changes in the adsorption isotherm, thereby generating artificial peaks in the pore size distribution, affecting the accuracy of the pore size distribution results. (Bardestani RPGSK S. Experimental methods in chemical engineering: specific surface area and pore size distribution measurements-BET, BJH, and DFT[J]. The Canadian Journal of Chemical Engineering, 2019, 97(11).) Therefore, while developing the gas adsorption method, we are also exploring new testing methods to truly restore the pore size distribution information of porous carbon.
[0042] Low-field NMR relaxation is a fast and non-destructive technique for studying the molecular dynamics of water in different pores (Li, Xiunan; Li, Yaqiong; Chen, Chao (2015). Pore size analysis from low field NMRspin–spin relaxation measurements of porous microspheres. Journal of Porous Materials, 22(1), 11–20. doi: 10.1007 / s10934-014-9864-x). The decay of the spin echo sequence (T2 relaxation time) measured by NMR is a function of the amount and distribution of hydrogen in the fluid, and is measured by recording the decrease in the spin echo amplitude over time. When water is in a porous material, its relaxation time is shorter than the relaxation time of water in free space due to the confinement effect.
[0043] The following 10 porous carbon samples were prepared and numbered Ⅰ to Ⅹ, and their physical and chemical data are shown in Table 1 below.
[0044] Table 1 Physical and chemical data of porous carbon samples
[0045]
[0046]
[0047] The pore size distribution of the above 10 porous carbon samples was tested by low-field nuclear magnetic resonance method:
[0048] (1) Test instrument: VTMR20-10V variable temperature nuclear magnetic resonance analyzer produced by Newmai Analytical Instrument Co., Ltd., with a resonance frequency of 21 MHz, a magnet temperature controlled at 32.00 ± 0.01 °C, and a probe coil diameter of 10 mm.
[0049] (2) Sample preparation (vacuum saturation): Add about 1 mL of water to a 2 mL mass spectrometer bottle (ensure that the water level is above the porous carbon sample after vacuum saturation and the pores are saturated with water), weigh the water (accurate to 0.0001 g), add the accurately weighed porous carbon sample (about 0.25 g, accurate to 0.0001 g, accounting for about 1 / 3 of the capacity of the mass spectrometer bottle), disperse it in water and continue to vacuum (-0.1 MPa) for 12 h.
[0050] (3) Sample testing: Liquid nitrogen was used to control the temperature of the sample chamber of the NMR analyzer to -6 ± 0.02 °C, and the water outside the pores was frozen. The NMR signal of the liquid water in the pores was tested. The NMR attenuation curve of the sample was plotted according to the relaxation time of the H atom resonance. The T2 spectrum of the sample was obtained after inversion and removal of the base. The low-field NMR T2 relaxation spectra of porous carbon samples V, VI, IX, and X are shown in Figure 2. Figure 2 As shown in the figure, the nitrogen adsorption isotherms corresponding to porous carbon samples V, VI, IX, and X are shown in the figure Figure 1 shown.
[0051] (4) Standard sample test: The result of NMR detection is a relative value, which needs to be calibrated using a low-temperature nano-porosity standard. Through a known calibration line, the NMR signal is linked to the mass of water in the pores to obtain the sample porosity.
[0052] (5) Result fitting: The porosity of the porous sample is calculated based on the mass of water in the pores obtained from the NMR signal and the compaction density and mass of the porous carbon (each group of samples is measured three times and the average value is taken as the result), and the lateral surface relaxation rate of the porous carbon (ρ, which is determined by the properties of the porous carbon itself and is set to ρ = 0.03 μm / s according to the pore size distribution corresponding to BET) is confirmed. Finally, the pore size distribution of porous carbon samples I to X is calculated based on the T2 spectrum of the sample saturated state without base inversion. The pore size distribution of porous carbon samples I to X is shown in the figure. Figures 4 to 13 As shown, the data are shown in Table 2.
[0053] Table 2 Low-field NMR pore size distribution of porous carbon
[0054]
[0055]
[0056] The pore size distribution of porous carbon is tested by NMR variable temperature analyzer. The NMR signal of H in the pores is tested under low temperature environment. According to the relaxation time of H atomic resonance in the pores, the NMR attenuation curve of the sample is drawn. After inversion, the pore size distribution differences of different porous carbon samples can be directly observed (such as Figure 2 This method can not only restore the pore size, but also quickly obtain a more accurate pore size distribution range (such as Figure 3 The pore size distribution curves of porous carbon sample Ⅶ measured by gas adsorption method and low-field nuclear magnetic resonance method are compared. It also has a simpler calculation method than the gas adsorption method. This method greatly reduces the test time while ensuring accuracy, and has good application prospects for the screening of porous carbon raw materials and their application in silicon-carbon negative electrode materials.
[0057] Example 1
[0058] Preparation of silicon-carbon negative electrode materials:
[0059] Porous carbon sample I was used as a porous carbon matrix. 12 kg of porous carbon sample I was placed in a fluidized bed, and nitrogen was introduced as a protective gas at a nitrogen flow rate of 21 L / min. The fluidized bed was heated to 500°C at a heating rate of 2°C / min. Monosilane was then introduced into the fluidized bed to deposit nanosilicon in the porous carbon. The monosilane gas flow rate was 35 L / min and the deposition time was 6 hours. After the deposition was completed, a deposited silicon porous carbon material was obtained. The reaction temperature was maintained at 500°C, and acetylene gas was introduced for carbon coating. The flow rate of acetylene gas was 15 L / min and the duration was 2 hours. A silicon-carbon negative electrode material was obtained. The material structure was based on a porous carbon matrix as the core, with a vapor-deposited nanosilicon material in the porous carbon matrix, and a carbon coating layer on the outer surface of the porous carbon matrix.
[0060] The silicon-carbon negative electrode material in this case is calculated based on 100% by weight: the vapor-deposited nano-silicon material accounts for 52.66wt%, the carbon coating layer accounts for 1.80wt%, and the remainder is the porous carbon matrix.
[0061] Example 2
[0062] Preparation of silicon-carbon negative electrode materials:
[0063] Porous carbon sample II was used as a porous carbon matrix. 12 kg of porous carbon sample II was placed in a fluidized bed, nitrogen was introduced as a protective gas, the nitrogen flow rate was 24 L / min, and the fluidized bed was heated to 400°C at a heating rate of 1°C / min; monosilane was then introduced into the fluidized bed, nano-silicon was deposited in the porous carbon, the monosilane gas flow rate was 40 L / min, the deposition time was 5 hours, and after the deposition was completed, a deposited silicon porous carbon material was obtained; the reaction temperature was maintained at 400°C, methane gas was introduced for carbon coating, the flow rate of methane gas was 15 L / min, and the duration was 2 hours, and a silicon-carbon negative electrode material was obtained, the material structure of which was based on a porous carbon matrix as the core, a vapor-deposited nano-silicon material in the porous carbon matrix, and a carbon coating layer on the outer surface of the porous carbon matrix.
[0064] The silicon-carbon negative electrode material in this case is calculated based on 100% by weight: the vapor-deposited nano-silicon material accounts for 48.77wt%, the carbon coating layer accounts for 1.07wt%, and the remainder is the porous carbon matrix.
[0065] Example 3
[0066] Preparation of silicon-carbon negative electrode materials:
[0067] Porous carbon sample III was used as a porous carbon matrix. 12 kg of porous carbon sample III was placed in a fluidized bed, and nitrogen was introduced as a protective gas at a nitrogen flow rate of 15 L / min. The fluidized bed was heated to 450°C at a heating rate of 4°C / min. Monosilane was then introduced into the fluidized bed to deposit nanosilicon in the porous carbon. The monosilane gas flow rate was 25 L / min and the deposition time was 8 hours. After the deposition was completed, a deposited silicon porous carbon material was obtained. The reaction temperature was maintained at 450°C, and ethylene gas was introduced for carbon coating. The flow rate of ethylene gas was 15 L / min and the duration was 2 hours. A silicon-carbon negative electrode material was obtained. The material structure was based on a porous carbon matrix as the core, with a vapor-deposited nanosilicon material in the porous carbon matrix, and a carbon coating layer on the outer surface of the porous carbon matrix.
[0068] The silicon-carbon negative electrode material in this case is calculated based on 100% by weight: the vapor-deposited nano-silicon material accounts for 50.79wt%, the carbon coating layer accounts for 1.62wt%, and the remainder is the porous carbon matrix.
[0069] Example 4
[0070] Preparation of silicon-carbon negative electrode materials:
[0071] Porous carbon sample IV was used as a porous carbon matrix. 12 kg of porous carbon sample IV was placed in a fluidized bed, nitrogen was introduced as a protective gas, the nitrogen flow rate was 12 L / min, and the fluidized bed was heated to 475°C at a heating rate of 5°C / min; monosilane was then introduced into the fluidized bed, nano-silicon was deposited in the porous carbon, the monosilane gas flow rate was 20 L / min, the deposition time was 10 hours, and after the deposition was completed, a deposited silicon porous carbon material was obtained; the reaction temperature was maintained at 475°C, propylene gas was introduced for carbon coating, the flow rate of propylene gas was 15 L / min, and the duration was 2 hours, and a silicon-carbon negative electrode material was obtained, the material structure of which was based on a porous carbon matrix as the core, a vapor-deposited nano-silicon material in the porous carbon matrix, and a carbon coating layer on the outer surface of the porous carbon matrix.
[0072] The silicon-carbon negative electrode material in this case is calculated based on 100% by weight: the vapor-deposited nano-silicon material accounts for 54.11wt%, the carbon coating layer accounts for 1.32wt%, and the remainder is the porous carbon matrix.
[0073] Example 5
[0074] Preparation of silicon-carbon negative electrode materials:
[0075] Porous carbon sample V was used as a porous carbon matrix. 12 kg of porous carbon sample V was placed in a fluidized bed, and nitrogen was introduced as a protective gas at a nitrogen flow rate of 10 L / min. The fluidized bed was heated to 525°C at a heating rate of 6°C / min. Monosilane was then introduced into the fluidized bed to deposit nanosilicon in the porous carbon. The monosilane gas flow rate was 16 L / min and the deposition time was 12 hours. After the deposition was completed, a deposited silicon porous carbon material was obtained. The reaction temperature was maintained at 525°C, and propylene gas was introduced for carbon coating. The flow rate of propylene gas was 15 L / min and the duration was 2 hours. A silicon-carbon negative electrode material was obtained. The material structure was based on a porous carbon matrix as the core, with a vapor-deposited nanosilicon material in the porous carbon matrix, and a carbon coating layer on the outer surface of the porous carbon matrix.
[0076] The silicon-carbon negative electrode material in this case is calculated based on 100% by weight: the vapor-deposited nano-silicon material accounts for 52.59wt%, the carbon coating layer accounts for 1.45wt%, and the remainder is the porous carbon matrix.
[0077] Example 6
[0078] Preparation of silicon-carbon negative electrode materials:
[0079] Porous carbon sample VI was used as a porous carbon matrix. 12 kg of porous carbon sample VI was placed in a fluidized bed, nitrogen was introduced as a protective gas, the nitrogen flow rate was 8 L / min, and the fluidized bed was heated to 550°C at a heating rate of 6°C / min; monosilane was then introduced into the fluidized bed, nano-silicon was deposited in the porous carbon, the monosilane gas flow rate was 14 L / min, the deposition time was 14 hours, and after the deposition was completed, a deposited silicon porous carbon material was obtained; the reaction temperature was maintained at 550°C, methane gas was introduced for carbon coating, the flow rate of methane gas was 15 L / min, and the duration was 2 hours, and a silicon-carbon negative electrode material was obtained, the material structure of which was based on a porous carbon matrix as the core, a vapor-deposited nano-silicon material in the porous carbon matrix, and a carbon coating layer on the outer surface of the porous carbon matrix.
[0080] The silicon-carbon negative electrode material in this case is calculated based on 100% by weight: the vapor-deposited nano-silicon material accounts for 45.58wt%, the carbon coating layer accounts for 2.11wt%, and the remainder is the porous carbon matrix.
[0081] Example 7
[0082] Preparation of silicon-carbon negative electrode materials:
[0083] Porous carbon sample Ⅶ was used as a porous carbon matrix. 12 kg of porous carbon sample Ⅶ was placed in a fluidized bed, and nitrogen was introduced as a protective gas at a nitrogen flow rate of 7.5 L / min. The fluidized bed was heated to 575°C at a heating rate of 10°C / min. Monosilane was then introduced into the fluidized bed to deposit nanosilicon in the porous carbon. The monosilane gas flow rate was 13 L / min and the deposition time was 15 hours. After the deposition was completed, a deposited silicon porous carbon material was obtained. The reaction temperature was maintained at 575°C, and ethylene gas was introduced for carbon coating. The flow rate of ethylene gas was 15 L / min and the duration was 2 hours. A silicon-carbon negative electrode material was obtained. The material structure was based on a porous carbon matrix as the core, with a vapor-deposited nanosilicon material in the porous carbon matrix, and a carbon coating layer on the outer surface of the porous carbon matrix.
[0084] The silicon-carbon negative electrode material in this case is calculated based on 100% by weight: the vapor-deposited nano-silicon material accounts for 52.23wt%, the carbon coating layer accounts for 1.98wt%, and the remainder is the porous carbon matrix.
[0085] Example 8
[0086] Preparation of silicon-carbon negative electrode materials:
[0087] Porous carbon sample VIII was used as a porous carbon matrix. 12 kg of porous carbon sample VIII was placed in a tubular furnace, and nitrogen was introduced as a protective gas at a nitrogen flow rate of 7 L / min. The tubular furnace was heated to 600°C at a heating rate of 5°C / min. Monosilane was then introduced into the tubular furnace to deposit nanosilicon in the porous carbon. The monosilane gas flow rate was 12 L / min and the deposition time was 16 hours. After the deposition was completed, a deposited silicon porous carbon material was obtained. The reaction temperature was maintained at 600°C, and propylene gas was introduced for carbon coating. The flow rate of propylene gas was 15 L / min and the duration was 2 hours. A silicon-carbon negative electrode material was obtained. The material structure was based on a porous carbon matrix as the core, with a vapor-deposited nanosilicon material in the porous carbon matrix, and a carbon coating layer on the outer surface of the porous carbon matrix.
[0088] The silicon-carbon negative electrode material in this case is calculated based on 100% by weight: the vapor-deposited nano-silicon material accounts for 44.45wt%, the carbon coating layer accounts for 3.06wt%, and the remainder is the porous carbon matrix.
[0089] Example 9
[0090] Preparation of silicon-carbon negative electrode materials:
[0091] Porous carbon sample IX was used as a porous carbon matrix. 12 kg of porous carbon sample IX was placed in a tube furnace, and nitrogen was introduced as a protective gas at a nitrogen flow rate of 6.5 L / min. The tube furnace was heated to 625°C at a heating rate of 5°C / min. Monosilane was then introduced into the tube furnace to deposit nanosilicon in the porous carbon. The monosilane gas flow rate was 11 L / min and the deposition time was 18 hours. After the deposition was completed, a deposited silicon porous carbon material was obtained. The reaction temperature was maintained at 625°C, and acetylene gas was introduced for carbon coating. The acetylene gas flow rate was 15 L / min and the duration was 2 hours. A silicon-carbon negative electrode material was obtained. The material structure was based on a porous carbon matrix as the core, with a vapor-deposited nanosilicon material in the porous carbon matrix, and a carbon coating layer on the outer surface of the porous carbon matrix.
[0092] The silicon-carbon negative electrode material in this case is calculated based on 100% by weight: the vapor-deposited nano-silicon material accounts for 56.43wt%, the carbon coating layer accounts for 2.58wt%, and the remainder is the porous carbon matrix.
[0093] Example 10
[0094] Preparation of silicon-carbon negative electrode materials:
[0095] A porous carbon sample X was used as a porous carbon matrix. 12 kg of porous carbon sample X was placed in a tube furnace, and nitrogen was introduced as a protective gas at a nitrogen flow rate of 6 L / min. The tube furnace was heated to 650°C at a heating rate of 5°C / min. Monosilane was then introduced into the tube furnace to deposit nanosilicon in the porous carbon. The monosilane gas flow rate was 10 L / min and the deposition time was 20 hours. After the deposition was completed, a deposited silicon porous carbon material was obtained. The reaction temperature was maintained at 650°C, and propylene gas was introduced for carbon coating. The flow rate of propylene gas was 15 L / min and the duration was 2 hours. A silicon-carbon negative electrode material was obtained. The material structure was based on a porous carbon matrix as the core, with a vapor-deposited nanosilicon material in the porous carbon matrix, and a carbon coating layer on the outer surface of the porous carbon matrix.
[0096] The silicon-carbon negative electrode material in this case is calculated based on 100% by weight: the vapor-deposited nano-silicon material accounts for 54.09wt%, the carbon coating layer accounts for 1.83wt%, and the remainder is the porous carbon matrix.
[0097] Manufacturing example
[0098] (1) Half-cell manufacturing:
[0099] The silicon-carbon negative electrode materials of the above embodiments were used to prepare negative electrode sheets, and button-type half-cells were assembled for testing, as follows:
[0100] Preparation of negative electrode sheet: The silicon-carbon negative electrode materials of the above embodiments were mixed with conductive additive carbon black and binder (sodium carboxymethyl cellulose and styrene-butadiene rubber in a mass ratio of 1:1) in a pulper at room temperature to prepare slurry. The prepared slurry was evenly coated on the copper foil, dried in a blast drying oven at 50°C for 2 hours, cut into 8mm diameter electrode sheets, and vacuum dried in a vacuum drying oven at 100°C for 10 hours. The dried electrode sheets were then transferred to the glove box for standby use for battery assembly.
[0101] Battery assembly: The simulated battery assembly was performed in a glove box containing a high-purity Ar atmosphere. Metallic lithium was used as the counter electrode, and 1 mol of LiPF 6 A solution formed in ethylene carbonate (EC) / dimethyl carbonate (DMC) (volume ratio v:v=1:1) was used as an electrolyte and a battery was assembled.
[0102] Half-cell test: A charge and discharge instrument was used to perform constant current charge and discharge mode testing. The discharge cut-off voltage was 0.005 V, the charge cut-off voltage was 1.5 V, and the charge and discharge test was performed at a current density of C / 10. The relevant test data obtained (charge specific capacity, first coulomb efficiency, etc.) are detailed in Table 3.
[0103] Table 3 Electrochemical performance of half-cells made of silicon-carbon negative electrode materials of various embodiments
[0104]
[0105] As shown in Table 3, the half-cell made of silicon-carbon negative electrode material with porous carbon matrix Ⅰ, Ⅱ, Ⅲ, Ⅳ, Ⅴ, Ⅵ, Ⅷ, Ⅸ as the core has a higher charge-discharge specific capacity and first efficiency, with the first efficiency of 1.5V reaching more than 90.5% and the first efficiency of 0.8V reaching more than 80%; while the battery made of silicon-carbon negative electrode material made of porous carbon matrix Ⅶ and Ⅹ has a first efficiency of only 75-78% at 0.8V. That is, the pore size distribution of the porous carbon matrix tested by low-field nuclear magnetic resonance in the present invention satisfies one of the following conditions: ① 0.2nm-7nm has a bimodal distribution; ② 1nm or less has a bimodal distribution, and there is one peak below 0.1nm and one peak between 0.1nm-1nm, so that a silicon-carbon negative electrode material with good electrochemical performance for lithium-ion batteries can be obtained.
[0106] (2) Full battery:
[0107] Referring to the preparation and testing process of the above half-cell, the silicon-carbon negative electrode material of each embodiment is used to prepare the negative electrode sheet, and the full battery is assembled and tested, as follows:
[0108] Preparation of positive electrode sheet: Formula parameters: 96.2wt% LiNi 0.6 Co 0.2 Mn 0.2 O 2 (622 positive electrode material) + 1.1wt% PVDF (binder) + 2.7wt% Super P (conductive agent); ingredient parameters: dry mixing, high-speed dispersion (solid content 72%), viscosity adjusted to about 5000cP for coating; coating parameters: single-sided surface density 21mg / cm 2 After being cut into 15 cm wide strips, the positive electrode sheets with a size of 73 mm × 44 mm were obtained by die cutting.
[0109] Preparation of negative electrode sheet: formula parameters: 95.0wt% negative electrode material (silicon-carbon negative electrode material of each embodiment) + 3.5wt% binder (sodium carboxymethyl cellulose and styrene-butadiene rubber in a mass ratio of 1:1) + 1.5wt% conductive agent carbon black; ingredient parameters: dry mixing and kneading (solid content 65%), high-speed dispersion (solid content 45%), viscosity adjustment to about 5000 for coating; coating parameters: single-sided surface density 9mg / cm 2 After being cut into 15 cm wide strips, the negative electrode sheets with a size of 75 mm × 46 mm were obtained by die cutting.
[0110] Assemble the battery: proceed as follows: stacking: stack 9 negative electrode sheets and 8 positive electrode sheets in a Z shape; welding the tabs: weld the tabs on the positive and negative electrodes respectively (positive electrode: aluminum; negative electrode: nickel); hot pressing and cold pressing: hot pressing at 80°C for 1 minute and cold pressing at room temperature for 1 minute; aluminum mold punching: the punching depth is 3mm; top sealing and side sealing: the heat sealing temperature is 190°C and the heat sealing time is 6 seconds; baking: keep warm at 95°C for 3 days, during which nitrogen replacement is performed to ensure that the sample is in an inert atmosphere; water content test: take about 1g of the positive electrode sheet and the negative electrode sheet, heat at 120°C to remove water, so that the moisture is less than 200ppm; injection: 1 mol of LiPF 6 The solution formed by ethylene carbonate (EC) / dimethyl carbonate (DMC) (volume ratio v:v=1:1) is used as the electrolyte and injected between the positive electrode plate and the negative electrode plate. The injection coefficient calculated according to the first charge is 3.5; sealing: heat sealing temperature is 190°C, heat sealing time is 3 seconds, and vacuum degree is -90; soak at 45°C for 2 days to obtain an assembled battery sample.
[0111] Full battery test: Cycle conditions: 1C / 1C; Voltage range: 2.8-4.25V.
[0112] The low temperature rate performance of lithium ion batteries made of the silicon-carbon negative electrode materials prepared in Example 1, Example 4, and Example 5 at -20°C is as follows: Fig.14 As shown, the lithium-ion battery made of the silicon-carbon negative electrode material prepared in Example 5 can maintain about 74% of its capacity at -20°C, the lithium-ion battery made of the silicon-carbon negative electrode material prepared in Example 4 can maintain about 69% of its capacity at -20°C, and the lithium-ion battery made of the silicon-carbon negative electrode material prepared in Example 1 can maintain about 70% of its capacity at -20°C. These three have good low-temperature rate performance. The present invention tests the pore size distribution of the porous carbon matrix through low-field nuclear magnetic resonance to meet one of the following conditions: ① 0.2nm-7nm has a bimodal distribution; ② 1nm or less has a bimodal distribution, and there is one peak below 0.1nm and one peak between 0.1nm-1nm, so that a silicon-carbon negative electrode material with good low-temperature rate performance for lithium-ion batteries can be obtained.
[0113] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A silicon-carbon negative electrode material for a lithium-ion battery, characterized in that: The structure of the silicon-carbon negative electrode material is based on a porous carbon matrix as the core, a vapor-deposited nano-silicon material is present in the porous carbon matrix, and a carbon coating layer is present on the outer surface of the porous carbon matrix; The silicon-carbon negative electrode material is calculated based on 100% by weight: the vapor-deposited nano-silicon material accounts for 30wt%-70wt%, the carbon coating layer accounts for 1wt%-5wt%, and the remainder is the porous carbon matrix; The pore size distribution of the porous carbon matrix measured by low-field nuclear magnetic resonance satisfies one of the following conditions: ①0.2nm-7nm has a bimodal distribution; ② There is a bimodal distribution below 1nm, with one peak below 0.1nm and one peak between 0.1nm-1nm; The total pore volume of the porous carbon matrix is 0.5 cm 3 / g or above, with a specific surface area of 1463m 2 / g or more; The oxygen content of the porous carbon matrix is between 0.5wt% and 3.0wt%; The method for preparing a silicon-carbon negative electrode material for a lithium-ion battery comprises the following steps: Porous carbon is added into a reaction container as a deposition substrate, protective gas is introduced to replace the air in the reaction container, and then the temperature is raised to a reaction temperature of 400°C-650°C, and silane gas is introduced at a flow rate of 10L / min-40L / min to vapor-deposit nano-silicon material in the porous carbon matrix for a deposition time of 5h-20h. After the deposition is completed, a deposited silicon porous carbon material is obtained; The reaction temperature is maintained, and then a gaseous carbon source is introduced at 1-20 L / min to carbon-coat the deposited silicon porous carbon material. The carbon coating time is 1-5 hours. After the reaction is completed, a silicon-carbon negative electrode material is obtained.
2. The silicon-carbon negative electrode material for lithium-ion batteries according to claim 1, characterized in that: The compaction density of the porous carbon matrix is 0.8 cm 3 / g -1.4 cm 3 / g; the particle size of the porous carbon matrix is between 0.1 microns and 40 microns, wherein the minimum particle size Dmin is between 0.1 microns and 2 microns, the average particle size D50 is between 5 microns and 10 microns, and the maximum particle size D100 is between 15 microns and 30 microns.
3. The silicon-carbon negative electrode material for a lithium-ion battery according to claim 1, characterized in that: The protective gas is nitrogen or argon, and the flow rate of the protective gas is 6L / min-24L / min; the heating rate is 1-10°C / min.
4. The silicon-carbon negative electrode material for a lithium-ion battery according to claim 1, characterized in that: The silane gas is selected from one or more of dichlorosilane, monosilane, disilane and trisilane; and the gaseous carbon source is selected from one or more of acetylene, methane, ethylene and propylene.
Citation Information
Patent Citations
Method for testing full pore size distribution of coal
CN114778405A
Multilayer composite material for secondary lithium ion battery as well as preparation method and application of multilayer composite material
CN116259726A
Preparation method and application of amorphous silicon-based negative electrode material
CN116281943A
Preparation method of silicon-carbon negative electrode material
CN116605875A
Three-dimensional porous silicon / carbon composite material, method for preparing same, and use thereof
US20220310989A1
Cited By
Silicon-carbon negative electrode material and preparation method and negative electrode sheet, lithium ion battery
CN122907628A