A polymer / nano zinc oxide composite film, preparation method and application

Through the composite film of polylactic acid, resin A and nano zinc oxide, combined with specific molar ratios and additive combinations, the poor mechanical properties and compatibility problems of biodegradable polymer plastics are solved, and a high-performance green antibacterial packaging material is achieved.

CN118165485BActive Publication Date: 2024-11-15JIYUAN LUTAI NANO MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410297913.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-15
Publication Date
2024-11-15
Estimated Expiration
2044-03-15

AI Technical Summary

Technical Problem

The existing biodegradable polymer plastics have problems in packaging materials such as poor mechanical properties, single properties, and poor compatibility with nano zinc oxide particles, which limits their application.

Method used

A composite film of polylactic acid, resin A and nano zinc oxide is prepared by a combination of specific molar ratios and additives, combined with melt granulation and casting methods, to improve the mechanical properties and antibacterial properties of the material.

Benefits of technology

It significantly improves the mechanical properties and antibacterial properties of the material, improves the dispersion between nano zinc oxide and polymer, enhances the barrier properties and antibacterial effects of the composite film, and is suitable for green and environmentally friendly packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004742881890000041
    Figure BDA0004742881890000041
  • Figure BDA0004742881890000051
    Figure BDA0004742881890000051
Patent Text Reader

Abstract

The present invention provides a polymer / nano zinc oxide composite film, a preparation method and an application. The composite film comprises, by weight, 60-80 parts of polylactic acid, 10-20 parts of resin A, 5-20 parts of nano zinc oxide and 5-10 parts of an auxiliary agent, wherein the resin A is a polymer formed by adipic acid, xylitol, ethylene glycol, 4,4'-stilbene dicarboxylic acid and a silicon hydride compound; the resin A is prepared by reacting adipic acid, xylitol, ethylene glycol, 4,4'-stilbene dicarboxylic acid and triethylsilane, and the resin A is compounded with a PLA resin, and nano zinc oxide is added at the same time, and the obtained polymer / nano zinc oxide composite film has good mechanical properties and good antibacterial properties, and well improves the problem of uneven dispersion when the polymer material is blended with the nano zinc oxide, and improves the performance defects existing when the polymer material is used as a packaging film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of green environmental protection packaging, and in particular to a polymer / nano zinc oxide composite film, a preparation method and application thereof. Background Art

[0002] Nano zinc oxide is a new type of multifunctional inorganic material with a particle size of about 1-100 nanometers. Due to the refinement of the grains, its surface electronic structure and crystal structure change, resulting in surface effects, volume effects, quantum size effects, macro tunneling effects, high transparency, high dispersibility and other characteristics that macroscopic objects do not have. In recent years, it has been found that it exhibits many special functions in catalysis, optics, magnetism, mechanics, etc., making it have important application value in many fields such as ceramics, chemical industry, electronics, optics, biology, medicine, etc., and has special features and uses that ordinary zinc oxide cannot compare with. Nano zinc oxide can be used for ultraviolet light shielding materials, antibacterial agents, fluorescent materials, photocatalytic materials, etc. Due to the series of advantages of nano zinc oxide and its very attractive application prospects, the research and development of nano zinc oxide has become the focus of many scientific and technological personnel.

[0003] With the continuous improvement of living standards, people's health awareness is gradually increasing, and their requirements for their living environment are getting higher and higher, which puts forward higher requirements for the safety and hygiene of packaging materials such as food and medicine. Since nano zinc oxide has antibacterial properties, its application in antibacterial packaging materials is the development trend of existing technology.

[0004] However, nano-oxides have a large specific surface area and high surface activity. Their high surface energy makes them easy to agglomerate and have poor dispersibility. After being mixed with organic polymer resins, they often cannot be well dispersed and easily form larger agglomerates, thereby reducing the nano effect of inorganic particles and greatly limiting their application.

[0005] Among biodegradable polymer plastics, biomass powder, polylactic acid (PLA), polycaprolactone (PCL), polyhydroxyalkyl ester (PHA), polybutylene adipate terephthalate (PBAT), polybutylene succinate (PBS) and polybutylene succinate adipate (PBSA) are currently used more. Among them, polylactic acid is obtained through biomass powder fermentation, monomer polymerization and other processes. It is a type of aliphatic polyester. Its mechanical properties are comparable to those of polyethylene terephthalate (PET) resin, but it is brittle and has a low heat deformation temperature, which requires special requirements for processing and molding equipment. Polyhydroxyalkyl esters can be synthesized by bioengineering or chemical engineering. Although the heat deformation temperature is high, it also has brittle defects and is difficult to blow mold into thin films. Other types of biodegradable polymer plastics may also have problems such as long degradation time and difficult processing. It can be seen that the current biodegradable polymer plastics may have problems such as long degradation time, high brittleness, poor mechanical properties, high processing difficulty, single performance, and comprehensive performance that cannot meet the requirements of actual applications.

[0006] Therefore, how to evenly mix nanoparticles with degradable polymer masterbatch and at the same time improve the mechanical properties and antibacterial properties of degradable polymer plastics is a key technology for the research and development of green antibacterial and degradable packaging materials. Summary of the invention

[0007] Purpose of the invention: The purpose of the present invention is to provide a polymer / nano zinc oxide composite film, a preparation method and an application, so as to solve the problems in the prior art that degradable polymer plastics as packaging materials have poor mechanical properties, single properties, and poor compatibility with inorganic nano zinc oxide particles, and promote development.

[0008] The technical solution of the present invention:

[0009] In one aspect, the present application provides a polymer / nano zinc oxide composite film, which comprises the following components by weight:

[0010] Polylactic acid 60-80 parts;

[0011] Resin A 10-20 parts;

[0012] Nano zinc oxide 5-20 parts;

[0013] 5-10 parts of additives;

[0014] The resin A is a polymer formed by adipic acid, xylitol, ethylene glycol, 4,4'-stilbene dicarboxylic acid and silicon hydride.

[0015] In some embodiments, the molecular weight or molecular weight distribution of the polylactic acid is not particularly limited as long as it can be substantially molded and processed, and the weight average molecular weight is preferably greater than 10,000, more preferably greater than 40,000. Optionally, the weight average molecular weight of the polylactic acid is 4w-8w.

[0016] In some embodiments, the particle size of the nano zinc oxide is not particularly limited, and any particle size range commonly used in the art can be used. Optionally, the particle size of the nano zinc oxide is 10-40 nm.

[0017] In some embodiments, the auxiliary agent is selected from one or more combinations of fillers, antioxidants, anti-blocking agents, antistatic agents, friction coefficient improvers, and colorants.

[0018] In some embodiments, the molar ratio of adipic acid, xylitol, ethylene glycol, 4,4'-stilbene dicarboxylic acid and silicon hydride is 5-10:1-2:8-15:3-5:3-5; preferably, the molar ratio of adipic acid, xylitol, ethylene glycol, 4,4'-stilbene dicarboxylic acid and silicon hydride is 10:2:12:3.5:3.

[0019] In some embodiments, the silicon hydride compound is selected from one or more combinations of dimethylsilane and trimethylsilane, monoethylsilane, diethylsilane, triethylsilane, monopropylsilane, dipropylsilane, tripropylsilane, monophenylsilane, diphenylsilane, triphenylsilane, phenylmethylsilane and phenylethylsilane, phenyldimethylsilane and phenyldiethylsilane, monomethoxysilane, dimethoxysilane and trimethoxysilane and monoethoxysilane, diethoxysilane and triethoxysilane, dimethylmethoxysilane, and methyldimethoxysilane.

[0020] In some embodiments, the method for preparing the resin A comprises:

[0021] S1: reacting 4,4'-stilbene dicarboxylic acid and a silicon hydride compound under the catalysis of a platinum catalyst to obtain a reaction product 1;

[0022] S2: Adipic acid, xylitol, ethylene glycol and reaction product 1 are mixed, a catalyst is added, and the mixture is heated for reaction to obtain resin A.

[0023] In some embodiments, the heating temperature of the heating reaction is 160-220°C.

[0024] In some embodiments, the polymer / nano zinc oxide composite film comprises the following components in parts by mass:

[0025] Polylactic acid 66-80 parts;

[0026] Resin A 15-20 parts;

[0027] Nano zinc oxide 5-12 parts;

[0028] 5-8 parts of additives.

[0029] On the other hand, the present application also provides a method for preparing the polymer / nano zinc oxide composite film, which specifically includes mixing the above raw materials, melt granulation, and preparing the film by casting method.

[0030] On the other hand, the present application also provides the use of the polymer / nano zinc oxide composite film as described above in packaging materials.

[0031] Beneficial effects:

[0032] Resin A was prepared by reacting adipic acid, xylitol, ethylene glycol, 4,4'-stilbene dicarboxylic acid and triethylsilane, and resin A was compounded with PLA resin, and nano zinc oxide was added. The obtained polymer / nano zinc oxide composite film had good mechanical properties and good antibacterial properties, which greatly improved the problem of uneven dispersion when polymer materials and nano zinc oxide were blended, and at the same time improved the performance defects of polymer materials when used as packaging films. DETAILED DESCRIPTION

[0033] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0034] Unless otherwise specified, the chemical reagents used in the present invention are all commercially available analytically pure.

[0035] Preparation of Resin A1

[0036] S1: 3.5 mol of 4,4'-stilbene dicarboxylic acid and 3 mol of triethylsilane were added to 100 ml of toluene solvent, 0.5 mol of platinum catalyst was added, and the mixture was reacted at 75° C. for 10 h to obtain reaction product 1;

[0037] S2: 5 mol of adipic acid, 1 mol of xylitol, 8 mol of ethylene glycol and 3 mol of reaction product 1 were mixed, 0.5 mol of concentrated sulfuric acid was added, and the mixture was heated at 110° C. for reaction. After washing, filtering and drying, resin A1 was obtained.

[0038] Preparation of Resin A2

[0039] The preparation method of resin A2 refers to that of resin A1, except that the molar ratio of adipic acid, xylitol, ethylene glycol and reaction product 1 is 10:2:15:3, and is recorded as resin A2.

[0040] Preparation of Resin A3

[0041] The preparation method of resin A3 refers to that of resin A1, except that the molar ratio of adipic acid, xylitol, ethylene glycol and reaction product 1 is 10:2:12:3.5, and is recorded as resin A3.

[0042] Preparation of Resin A4

[0043] The preparation method of resin A4 refers to that of resin A1, except that the molar ratio of adipic acid, xylitol, ethylene glycol and reaction product 1 is 10:0:14:3.5, and is recorded as resin A4.

[0044] Preparation of Resin A5

[0045] Adipic acid, xylitol, ethylene glycol and 4,4'-stilbene dicarboxylic acid were mixed, 0.5 mol of concentrated sulfuric acid was added, heated at 110°C for reaction, washed, filtered and dried to obtain resin A5. The molar ratio of adipic acid, xylitol, ethylene glycol and 4,4'-stilbene dicarboxylic acid was 10:2:12:3.5.

[0046] Preparation of Resin A6

[0047] Adipic acid and ethylene glycol were mixed, 0.5 mol of concentrated sulfuric acid was added, and the mixture was heated at 110° C. for reaction, and then washed, filtered, and dried to obtain resin A6. The molar ratio of adipic acid to ethylene glycol was 1:1.

[0048] Examples 1-5 and Comparative Examples 1-4

[0049] Polylactic acid, the resin A, nano zinc oxide, antioxidant 1010 and calcium stearate were uniformly mixed, and extruded and granulated by a forward extrusion twin-screw extruder to prepare a series of polymer / nano zinc oxide composite blended granules.

[0050] The raw materials of the above pellets are shown in Table 1.

[0051] Table 1 Formula table of Examples 1-5 and Comparative Examples 1-3

[0052]

[0053] Note: In the above table, "L" indicates an example, such as "L1" indicates Example 1; "D" indicates a comparative example, such as "D1" indicates Comparative Example 1. The average weight average molecular weight of polylactic acid is 80,000. The particle size of nano zinc oxide is 30 nm.

[0054] The series of polymer / nano zinc oxide composite blended granules obtained above were vacuum dried at 50° C. for 24 h, and composite membranes were prepared by a cast film machine to obtain composite membranes 1-8 in sequence.

[0055] The above composite films 1-8 were subjected to the following performance tests, and the test results are shown in Table 2:

[0056] 1. Mechanical properties: Tested in accordance with GB / T 1040.2-2022 standard, with a tensile rate of 20 mm / min and an experimental temperature of 25 °C.

[0057] 2. Antibacterial performance: According to QB / T 2591-2003 "Test Methods and Antibacterial Effects of Antibacterial Plastics", the test bacteria are Escherichia coli ATCC 25922 and Staphylococcus aureus ATCC 6538. The test steps are as follows: Disinfect the sample to be tested with 75% ethanol and dry it, dilute the strain with sterile water to a bacterial suspension of appropriate concentration for use. Take 0.2mL of the bacterial suspension and drop it on the surface of the sample, cover it with a 0.1mm thick composite film (4.0cm×4.0cm), so that the bacterial suspension forms a uniform liquid film between the sample and the film. Keep the relative humidity at 90% at 37℃ for 18 hours. Wash the bacterial solution with sterile water, dilute it into an appropriate concentration gradient, and take 0.1mL and evenly spread it on the prepared sterile agar medium. Incubate at 37℃ for 18 hours and observe the results. The blank control is replaced by a sterile plate, and the other operations are the same.

[0058] 3. Barrier performance: Oxygen permeability is tested in accordance with GB / T 19789-2005.

[0059] Table 2 Experimental test results

[0060]

[0061] It can be seen from the above table that the synergistic effect between the components of the composite film prepared by the present invention can produce a good interface bonding effect, improve the problem of uneven dispersion when the polymer material and nano zinc oxide are blended, thereby enhancing the mechanical properties of the composite material and showing good barrier and antibacterial properties.

[0062] The addition of xylitol can increase the cross-linking degree of resin A, improve the mechanical properties and barrier properties of the composite film, and at the same time, controlling the amount of xylitol added can make the film have the characteristics of high hardness and good toughness, making it suitable for use as a packaging product.

[0063] The nano zinc oxide and the resin A work together to improve the antibacterial property of the film composition, so that the antibacterial rate of the film against Escherichia coli and Staphylococcus aureus can reach 99.9%.

[0064] The present invention can also have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.

Claims

1. A polymer / nano zinc oxide composite film, It is characterized in that In parts by mass, it includes the following components: Polylactic acid 60-80 parts; Resin A 10-20 parts; Nano zinc oxide 5-20 parts; 5-10 parts of additives; Wherein, the resin A is a polymer formed by adipic acid, xylitol, ethylene glycol, 4,4'-stilbene dicarboxylic acid and silicon hydride; The silicon hydride compound is triethylsilane.

2. According to claim 1, the polymer / nano zinc oxide composite film, It is characterized in that The molar ratio of the adipic acid, xylitol, ethylene glycol, 4,4'-stilbene dicarboxylic acid and silicon hydride is 5-10: 1-2: 8-15: 3-5: 3-5.

3. The polymer / nano zinc oxide composite film according to claim 1, It is characterized in that The molar ratio of the adipic acid, xylitol, ethylene glycol, 4,4'-stilbene dicarboxylic acid and silicon hydride is 10:2:12:3.5:

3.

4. The polymer / nano zinc oxide composite film according to claim 1, It is characterized in that The preparation method of the resin A comprises: S1: reacting 4,4'-stilbene dicarboxylic acid and a silicon hydride compound under the catalysis of a platinum catalyst to obtain a reaction product 1; S2: Adipic acid, xylitol, ethylene glycol and reaction product 1 are mixed, a catalyst is added, and the mixture is heated for reaction to obtain resin A.

5. The polymer / nano zinc oxide composite film according to claim 1, It is characterized in that The polymer / nano zinc oxide composite film comprises the following components in parts by mass: Polylactic acid 66-80 parts; Resin A 15-20 parts; Nano zinc oxide 5-12 parts; 5-8 parts of additives.

6. The polymer / nano zinc oxide composite film according to claim 1 or 5, It is characterized in that The weight average molecular weight of the polylactic acid is 4w-8w; the particle size of the nano zinc oxide is 10-40nm.

7. The polymer / nano zinc oxide composite film according to claim 1 or 5, It is characterized in that The auxiliary agent is selected from one or more combinations of fillers, antioxidants, anti-blocking agents, antistatic agents, friction coefficient improvers, and colorants.

8. The method for preparing the polymer / nano zinc oxide composite film according to any one of claims 1 to 7, It is characterized in that The method comprises the steps of mixing the above raw materials, melting granulation and preparing the composite film by a casting method.

9. Use of the polymer / nano zinc oxide composite film according to any one of claims 1 to 7 in packaging materials.

Citation Information

Patent Citations

  • Antibacterial polylactic acid film material

    CN109111702A

  • Bio-based antibacterial packaging film and preparation method thereof

    CN115710409A

  • Degradable polylactic acid special-purpose toughening hydrophilic master batch and preparation method thereof

    CN115746571A

  • Antibacterial polylactic acid resin composition and antibacterial composite resin material containing the same

    JP2022090392A

  • Biodegradable polyester resin composition containingnano particles

    KR1020060003580A