A room temperature cured high-toughness cavitation-resistant polyurethane coating and preparation method thereof
A room temperature curing polyurethane coating with optimized components and a two-stage temperature control method addresses the limitations of high-temperature vulcanization, providing high strength, toughness, and cavitation resistance for large and complex components.
Patent Information
- Application Number
- CN202410311490.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-19
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-03-19
AI Technical Summary
Existing polyurethane coatings for protecting ship propellers and turbine units from cavitation require high-temperature vulcanization processes, professional equipment, and are not suitable for large or complex shapes, leading to poor mechanical properties and inadequate cavitation resistance.
A room temperature curing process is developed using a two-stage temperature control method and optimized components, including aromatic polyisocyanate and triol crosslinking agents, to produce a polyurethane coating with high reactivity and viscosity, ensuring excellent bonding and cavitation resistance.
The coating achieves high strength, toughness, and hydrolysis resistance, effectively resisting cavitation on large and complex components with minimal environmental impact, suitable for ship propellers and turbines.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to a room temperature cured high-toughness cavitation-resistant polyurethane coating and a preparation method thereof, belonging to the technical field of coatings and protective coatings. Background Art
[0002] Since the beginning of the 21st century, my country has seen a large gap in high-performance ships, and it is urgent to carry out targeted reinforcement in terms of ship tonnage, speed and other performance. This has put forward extremely high requirements on the research and development and manufacturing technology of my country's shipbuilding industry. One of the difficulties is the serious cavitation damage faced by propellers, rudders and other ship propulsion devices and appendages. At the same time, in order to achieve the "dual carbon goals", my country has been vigorously developing new green energy based on hydropower in the Yangtze River, Yellow River and other basins in the central and western regions. However, the serious cavitation problem of turbine units has significantly reduced the output efficiency of the equipment, and may even cause long-term shutdowns for maintenance, seriously affecting the development and utilization of clean energy. Therefore, the development of protective materials with excellent anti-cavitation performance is of great practical and economic significance.
[0003] Since cavitation damage starts from the surface of the component, using surface technology to coat the surface of the component with a layer of cavitation-resistant coating material is undoubtedly a more economical and feasible way. The invention patent with publication number CN115418595B, "A high entropy alloy coating that resists cavitation-corrosion and its preparation method", uses supersonic flame spraying technology to prepare an Al-Cr-CoNi series high entropy alloy coating on the surface of a metal substrate that can absorb mechanical impact energy through plastic deformation, showing very good anti-cavitation-corrosion performance, but the coating relies on supersonic flame spraying equipment, and it is difficult to perform on-site construction on propellers, rudders or turbines with a size of several meters in the field. Compared with high entropy alloys that absorb impact energy through plastic deformation, elastic polyurethane with a microphase separation structure receives the load impact released by bubble collapse with hard segment molecular chains and transmits it to soft segment molecular chains, and then dissipates it through the latter's flexible movement, which obviously has a better energy absorption effect. The invention patent "A polyurethane elastomer" with the publication number CN103012736 A discloses a method for preparing a polyurethane elastomer with a flexion number of more than 200,000 times. However, its preparation process requires the use of a reduced pressure vacuum environment and two vulcanization processes with a temperature exceeding 100°C. It still requires professional equipment such as an oven, resulting in poor construction performance on the surface of large and special-shaped flow-through parts, making it difficult to use as an anti-cavitation coating. The invention patent "Anti-cavitation topcoat and its preparation method and application" with the publication number CN116218347B discloses a method for preparing a polyurethane elastomer with diisocyanate, polyether diol and polytetrafluoroethylene as the main raw materials. Although a high-temperature vulcanization process is not required, the mechanical properties of the material are low and further enhancement by carbon nanotubes, silicon carbide, etc. is required, which not only increases the cost, but also the cavitation resistance of the prepared coating is still poor. The cumulative mass loss of cavitation for 20 hours is as high as 24~50 mg, which is difficult to meet the cavitation protection requirements of new ships and turbine units. Summary of the invention
[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing a high-strength and tough cavitation-resistant polyurethane coating that cures at room temperature, so as to better coat the surfaces of large flow-through components such as ship propellers, appendages and turbines, and achieve better cavitation protection effects.
[0005] The present invention optimizes the type, molecular weight and molar ratio of polyisocyanate and polyol, and selects a two-stage temperature rise and temperature control process to control the reaction rate and reaction mode between the two, thereby ensuring the production of high-quality -NCO-terminated prepolymer (component A). The strong electron-withdrawing effect of the benzene ring in the aromatic polyisocyanate, the electron cloud and distribution state of the -NCO group, can also give the prepolymer higher reactivity and smaller steric hindrance, thereby avoiding the disadvantage of using an organic metal catalyst when reacting with component B, making the production process simpler and greener. By optimizing the type, addition content and addition method of the triol crosslinking agent, especially the chlorine-containing aromatic diamine small molecule chain extender (component B), and selecting a temperature gradient reaction method, the reactivity of the amino group in component B can be moderately reduced, the generation of by-products in the reaction process between component B and component A can be significantly reduced, and the production of polyurethane coatings with moderate reactivity and viscosity and moderate excess of -NCO can be ensured. Moderate curing time and viscosity are not only conducive to the long-term application process of the coating on the surface of large parts, but also can promote sufficient wetting between the resin and the substrate surface, which is conducive to improving the bonding strength of the coating. The optimized components, especially the sufficient chemical cross-linking and the moderately excessive -NCO groups, can also ensure that after the coating is applied to the surface of the metal substrate, while -NCO reacts with water molecules in the air, -NHCONH- and -NHCO- form hydrogen bonds with the -OH active groups exposed on the surface of the substrate, and finally achieve room temperature curing and obtain a polyurethane coating with high binding, high fracture strength, high elongation at break, high toughness, and excellent hydrolysis resistance. The cavitation resistance of the polyurethane coating in water is not only significantly better than that of metal materials commonly used in flow-through parts such as L907A steel, but also significantly better than other publicly available polyurethane coatings, and has obvious advantages in being used as a cavitation-resistant coating on the surface of large and special-shaped parts such as propellers, rudders and turbines.
[0006] 1. Preparation of polyurethane coating
[0007] The preparation of the polyurethane coating of the present invention comprises the following process steps:
[0008] (1) Preparation of NCO-terminated prepolymer
[0009] Add aromatic polyisocyanate dissolved in butyl acetate to the preheated polyol, and adopt a two-stage temperature control method to react. First, slowly heat up to 35-35°C, stir for 5-20 minutes, then continue to heat up to 75-80°C, stir for 2-3 hours to obtain the prepolymer, which should be sealed and stored at low temperature.
[0010] The aromatic polyisocyanate is selected from one or more of toluene diisocyanate (TDI) and diphenylmethane-4,4'-diisocyanate (MDI). The polyol molecular weight is polytetramethylene ether diol (PTMG) of 2000-3000. The molar ratio of -NCO in the aromatic polyisocyanate to the hydroxyl group in the polyol (-NCO:-OH) is 2.4-2.1:1.
[0011] In order to verify whether the reaction between polyol and polyisocyanate is completed, the residual isocyanate content in the solution is calibrated according to the method of Chinese chemical industry standard HG / T2409-1992 "Determination of isocyanate content in polyurethane prepolymer": the mass percentage of isocyanate group is calculated by titrating the di-n-butylamine remaining after the isocyanate group reacts with the scalar di-n-butylamine with hydrochloric acid, and the reaction is stopped when the -NCO mass fraction reaches the theoretical value.
[0012] The prepolymer solution was coated on a potassium bromide salt sheet and observed by Fourier transform infrared spectroscopy (FTIR) using a smear method. The scanning background was potassium bromide salt sheet and air. The infrared spectrometer used was Brukervertex 70. Figure 1 is the infrared spectrum of the prepolymer, a is the infrared spectrum curve of PTMG, and b is the infrared spectrum curve of the prepolymer. Figure 1 It shows that after the reaction, the b curve at 3469 cm -1 The -OH stretching vibration peak at 3320 cm -1 The -NH- stretching vibration peak appears at 2270cm -1 The -NCO stretching vibration peak appears at 1740 cm -1 The C=O stretching vibration peak of -NHCO- appears at , indicating that -OH reacts with -NCO to form a carbamate group (-NHCO-), proving the successful synthesis of the -NCO-terminated prepolymer and obtaining the target prepolymer.
[0013] (2) Preparation of coating
[0014] Add butyl acetate to the prepolymer and preheat to 25-35°C as component A; preheat and dissolve the triol crosslinking agent and the chlorine-containing aromatic amine small molecule chain extender with a solvent as component B; add component B to component A, mix evenly, and react according to the temperature gradient within 30-70°C: slowly heat to 30-40°C, keep warm for 5-15 min; slowly heat to 40-48°C, keep warm for 5-25 min; slowly heat to 48-70°C, keep warm for 5-30 min. During this period, take out a small amount of solution and titrate it with di-n-butylamine until the -NCO content reacts to the theoretical value, stop the reaction, add small molecule additives, mix evenly, and obtain the polyurethane coating.
[0015] The triol crosslinking agent is selected from one or more of trimethylolpropane (TMP) and trimethylolethane (TME). The chlorine-containing aromatic amine small molecule chain extender is selected from one or more of 3,3'-dichloro-4,4'-diaminodiphenylmethane (MOCA) and 4,4'-methylenebis(3-chloro-2,6-diethylaniline) (MCDEA). The total molar ratio (-NCO: -OH+-NH2) of the isocyanate group of the prepolymer in component A to the hydroxyl group (hydroxyl group in the triol crosslinking agent) and amino group (amino group in the chlorine-containing aromatic amine small molecule chain extender) in component B is 1.03~1.10:1. The small molecule auxiliary agent is a defoaming agent.
[0016] (3) Application of coating
[0017] First, the surface of the metal substrate is sandblasted to remove surface dirt, rust, etc., and the rust removal level is at least Sa 2.5. Then, the diluted polyurethane coating is applied to the surface of the substrate by brushing, scraping, dipping, rolling or spraying. The application time is controlled at 0.5~3h and the thickness is controlled at 1~3mm.
[0018] The metal substrate is one of stainless steel, nickel aluminum bronze, L907A steel, cast steel, carbon steel, and titanium alloy. The solid content of the diluted polyurethane coating is ≥20%.
[0019] (4) Curing of coating
[0020] Place the substrate coated with polyurethane coating in the room temperature atmosphere for 5 to 10 days to complete moisture curing. The room temperature curing temperature range is 10~40℃.
[0021] In order to track the curing degree of the polyurethane coating, the coating cured on the release paper was observed by Fourier transform infrared spectroscopy (FTIR) using attenuated total reflection (ATR) using a Bruker vertex 70 infrared spectrometer. -1When the peak representing the isocyanate group disappears, curing is considered complete. If the peak still exists, the curing time should be appropriately extended. Figure 2 This is the infrared spectrum of the coating after curing for 7 days in Example 2. The visible wavelength is 2270 cm -1 The -NCO stretching vibration peak disappears, proving that the curing of the polyurethane coating is complete.
[0022] 2. Structure and properties of polyurethane coating
[0023] 1. Microphase separation structure of polyurethane coating
[0024] Polyurethane elastomers have a unique microphase separation structure due to the thermodynamic incompatibility between hard segments and soft segments, including amorphous soft segments and partially crystalline hard segments, which gives them good mechanical properties such as strength and elasticity. Within a certain range, the greater the degree of microphase separation, the greater the ability of polyurethane to absorb mechanical impact energy and resist external impact. The microphase separation degree of the polyurethane coating of the present invention was characterized using a Bruker small angle X-ray scattering instrument (SAXS), and the detector was Pilatus 3R300K. Figure 3 SAXS spectra of the coatings prepared in Example 2 and Comparative Example 1 (the type of solvent is not within the scope specified in the claims of the invention). The visible scattering vector is 0.5 nm -1 At , Example 2 shows a stronger peak, that is, the degree of microphase separation in Example 2 is greater than that in Comparative Example 1. The difference is mainly due to the excessive polarity of the solvent used in Comparative Example 1, which causes the strong polar groups such as carbamate groups and urea groups contained in the hard segment to be too dispersed, which is not conducive to crystallization and reduces the degree of microphase separation. In Example 2, the polarity of the preferred solvent is more moderate, which promotes the crystallization of the hard segment, makes the hard segment more easily aggregated into micro-regions dispersed in the soft segment, increases the degree of microphase separation, and can play a reinforcing role similar to that of fillers, which is beneficial to the improvement of the mechanical properties and anti-cavitation properties of the polyurethane.
[0025] 2. Mechanical properties of polyurethane coating
[0026] The mechanical properties of the polyurethane coating were evaluated by tensile testing using a universal tensile testing machine. The coating samples were cured on release paper and cut into dumbbell-shaped specimens using a cutter. Figure 4 to Figure 7 Figure 2 is the stress-strain curve obtained by tensile test of different coatings. It can be seen that the fracture strength of the coatings prepared in Example 1, Example 2, and Example 3 (within the scope of the claims of the present invention) are 51.92 MPa, 55.26 MPa, and 47.56 MPa, respectively, the elongation at break are 905%, 811%, and 869%, respectively, and the toughness is 199.24 MJ m -3 , 195.60 MJ m -3 and 167.82 MJ m-3 The coatings prepared in Comparative Example 1 (the type of solvent is not within the scope of the invention claims), Comparative Example 2 (the types of solvent, polyisocyanate and chain extender and the molecular weight of polyol are not within the scope of the invention claims) and Comparative Example 3 (the synthesis method is not within the scope of the invention claims) have a breaking strength of 37.28 MPa, 25.42 MPa and 2.18 MPa, respectively, a breaking elongation of 916.01%, 1175.22% and 107.98%, and a toughness of 132.52 MJ m -3 , 93.80 MJ m -3 and 20.57MJ m -3 Obviously, the polyurethane coating material obtained by using the technical solution of the present invention has significantly better comprehensive mechanical properties and has the remarkable characteristics of high strength and toughness, which is beneficial to resist the impact of mechanical energy released by bubble collapse and improve the cavitation resistance of the coating.
[0027] In addition, the elasticity of the polyurethane coating was evaluated using a GT-7042-REA resilience tester in accordance with GB / T 1681-2009. The test results showed that the polyurethane coating prepared by the present invention had good elasticity, ranging from 40% to 60%, which was closely related to its larger degree of microphase separation.
[0028] The bonding strength of the polyurethane coating was evaluated using a universal tensile testing machine. The test results showed that the bonding strength between the polyurethane coating prepared in the present invention and commonly used metal substrates of flow-through components such as L907A steel and carbon steel was higher than 7 MPa, which can well meet the needs of practical applications.
[0029] 3. Water absorption and hydrolysis stability of polyurethane coating
[0030] The polyurethane materials prepared in Example 1, Example 2, Example 3 and Comparative Example 2 were cut into blocks with a size of approximately 15 mm×15 mm×2 mm, and then the blocks were immersed in deionized water at room temperature. The mass changes of the blocks after immersion for a certain period of time were recorded using a 1 / 10,000 balance until the mass stabilized.
[0031] Figure 8 The following are line graphs showing the water absorption rate of the polyurethanes prepared in Example 1, Example 2, Example 3 and Comparative Example 2 at room temperature over time. It can be seen that the water absorption rate of the polyurethane coating of the present invention is significantly lower than that of Comparative Example 2, both of which are less than 2%, which is mainly attributed to the fact that the preferred types and ratios of the crosslinking agent and chain extender in the present invention greatly increase the crosslinking density of the polyurethane coating, making the polyurethane molecular network denser, which can effectively prevent and delay the penetration of water molecules.
[0032] In order to test the hydrolytic stability of the coating, the present invention takes Example 2 as an example. After the sample is immersed in deionized water at room temperature for 480 h, the molecular chain structure changes of the coating are observed using a Fourier transform infrared spectrometer (FTIR) and an attenuated total reflectance method (ATR). The scanning background is air, and the infrared spectrometer used is a Bruker vertex 70.
[0033] Fig. 9 The original infrared spectrum (a) of the polyurethane coating prepared in Example 2 and the infrared spectrum (b) after immersion for 480 hours, Fig.10 1550~1800 cm -1 After 480 h of immersion, the full spectrum, especially the most hydrolyzed 1740 cm -1 The C=O stretching vibration peak of -NHCO- at 1640 cm -1 The absorption intensity of the C=O stretching vibration peak of -NHCONH- at NHCONH- did not show obvious change, which proves that the polyurethane coating synthesized in the present invention has excellent hydrolysis resistance.
[0034] The ultra-low water absorption and excellent hydrolysis resistance of the polyurethane coating of the present invention play a very important role in its use as an underwater anti-cavitation coating.
[0035] 4. Anti-cavitation performance of coating
[0036] In order to better study the cavitation performance of polyurethane coating, the coating samples were subjected to accelerated cavitation experiments using an ultrasonic vibration cavitation tester that complies with the GB / T 6383-2009 standard. The conditions of the accelerated cavitation test are as follows: the diameter of the upper sample end face is 16 ± 0.02 mm, the vibration frequency is 20 kHz, and the amplitude is 50 μm (peak-to-peak); the coating sample is fixed on the sample table as the lower sample, with a distance of 0.5 ± 0.05 mm from the upper sample and 12.0 ± 1.0 mm from the liquid surface; the liquid medium is deionized water, and the water temperature is controlled at 25 ± 2 ℃ by a circulating temperature control system. The mass of the coating before and after a certain period of cavitation is weighed using a one-tenth of a balance, and the cumulative mass loss is the difference between the two.
[0037] Under the same conditions, after cavitation for 80 h, the cumulative mass loss of Example 1 is 0.8 mg, Example 2 is 0.4 mg, and Example 3 is 0.6 mg. The cavitation resistance of Example 1 is significantly better than that of L907A steel (69.7 mg) after cavitation for 10 h, Comparative Example 1 (6.9 mg) after cavitation for 80 h, Comparative Example 2 (9.8 mg) after cavitation for 30 h, and Comparative Example 3 (9.5 mg) after cavitation for 6 h. Fig.11 and Fig.12The following are photos of the appearance of Example 2 and Comparative Example 3 after cavitation for a period of time. It can be seen that extremely serious fatigue cracks appeared on the surface of Comparative Example 3 after only 6 hours of cavitation, and the cracks have longitudinally extended to the interface between the coating and the substrate, resulting in the separation of the coating and the substrate in the cavitation area, the appearance of "bulging", and extremely poor cavitation resistance; on the contrary, the coating prepared in Example 2 remained intact on the surface after cavitation for up to 240 hours. The above data show that the polyurethane coating of the present invention can well mitigate and resist the mechanical impact caused by the collapse of bubbles, and has excellent cavitation resistance. When the type of solvent, polyisocyanate or chain extender, molecular weight or synthesis method of polyol, etc. are not within the scope specified in the claims of the present invention, the cavitation resistance of the coating will be significantly reduced.
[0038] In summary, the present invention optimizes the use of moderately excessive -NCO groups and aromatic polyisocyanates with less steric hindrance as hard segment components, and uses polyols with higher molecular weight as soft segment components, which can not only avoid the shortcomings of traditional polyurethane coatings that rely on organic metal catalysts during the production process, making the production process simpler and greener, but also give the polyurethane coating higher strength, tensile strength and toughness. By optimizing the use of chlorine-containing aromatic diamine small molecules with moderate reaction activity as chain extenders, as well as the addition ratio of chain extenders and crosslinkers, and adopting a temperature gradient reaction process, the formation of reaction by-products can be effectively avoided, and the polyurethane coating is given a more suitable viscosity, curing time and curing conditions, effectively avoiding the curing process of high-temperature vulcanization that traditional polyurethane coatings usually require, which can not only better ensure the construction of thick coatings on the surface of large parts, but also effectively increase the wettability and bonding strength between the coating and the metal substrate. More importantly, the above-mentioned structural properties also give the polyurethane coating of the present invention extremely low water absorption underwater and extremely high hydrolysis resistance and cavitation resistance. Therefore, the room temperature curing high-toughness polyurethane coating of the present invention will have better protection ability and application prospects whether on the surface of ship propellers and appendages or on the surfaces of components such as turbines and impellers. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 Infrared spectra of raw materials and prepolymers.
[0040] Figure 2 This is the infrared spectrum of Example 2 after curing.
[0041] Figure 3 The SAXS spectra of the polyurethanes prepared in Example 2 and Comparative Example 1 are shown.
[0042] Figure 4 The strain-stress tensile curve of the polyurethane prepared in the example.
[0043] Figure 5This is the strain-stress tensile curve of the polyurethane prepared in Comparative Example 1.
[0044] Figure 6 This is the strain-stress tensile curve of the polyurethane prepared in Comparative Example 2.
[0045] Figure 7 This is the strain-stress tensile curve of the polyurethane prepared in Comparative Example 3.
[0046] Figure 8 The water absorption curve of the polyurethane prepared in Example and Comparative Example 2 changes with time.
[0047] Fig. 9 Comparison of infrared spectra of the polyurethane coating prepared in Example 2 before and after soaking in water.
[0048] Fig.10 This is a partial enlarged view of the infrared spectrum of the polyurethane coating prepared in Example 2 before and after soaking in water.
[0049] Fig.11 This is a photograph of the appearance of the polyurethane coating prepared in Example 2 after cavitation for 240 hours.
[0050] Fig.12 This is a photograph of the appearance of the polyurethane coating prepared in Comparative Example 3 after cavitation for 6 hours. DETAILED DESCRIPTION
[0051] In order to enable those skilled in the art to better understand the technical solution of the present invention, the preparation of the room temperature curing high-toughness cavitation-resistant polyurethane coating of the present invention is further described below in conjunction with implementation cases.
[0052] Example 1
[0053] (1) Preparation of -NCO-terminated prepolymer: Add 51.15 g of polytetrahydrofuran ether diol (Mn=2000) into a three-necked flask, preheat to 30°C, and then add 10.00 g of toluene diisocyanate dissolved in 5.0 mL of butyl acetate under nitrogen protection at a drop rate of about 2 drops / second. After stirring evenly, slowly heat to 40°C, stir for 10 min, and then heat to 80°C. After reacting for 2.5 h, the theoretical value is reached to obtain the prepolymer, stop the reaction, and store in a sealed container at low temperature.
[0054] (2) Preparation of coating: Add 8.0 mL of butyl acetate to the above prepolymer and preheat to 30°C to obtain component A. Heat and dissolve 6.83 g of 3,3'-dichloro-4,4'-diaminodiphenylmethane and 0.26 g of trimethylolpropane in 9.5 mL of butyl acetate to obtain component B. Add component B to component A, stir evenly, and react at a temperature gradient within 30-70°C: slowly heat to 30-40°C and keep warm for 10 min; slowly heat to 40-48°C and keep warm for 15 min; slowly heat to 48-70°C and keep warm for 15 min. After the reaction reaches the theoretical value of the -NCO mass fraction, stop the reaction, add a defoamer, and mix evenly to obtain a polyurethane coating.
[0055] (3) Application of coating: First, the stainless steel surface is sandblasted to remove dirt, rust, etc. on the surface, and the rust removal level reaches Sa 2.5. Then, the polyurethane coating with a diluted solid content of 80% is applied to the surface of the stainless steel substrate by brushing. The application time is up to 1 hour and the thickness is about 2 mm.
[0056] (4) Curing of coating: Place the stainless steel substrate coated with polyurethane coating in an atmospheric environment at room temperature of 15-25°C for 7 days to complete moisture curing.
[0057] (5) Cavitation resistance of the coating: Under the aforementioned accelerated cavitation test conditions, the cumulative mass loss of the coating was 0.8 mg after cavitation for 80 h.
[0058] Example 2
[0059] (1) Preparation of -NCO-terminated prepolymer 51.15 g of polytetrahydrofuran ether diol (Mn=2000) was added to a three-necked flask and preheated to 30°C. Then, 10.00 g of toluene diisocyanate dissolved in 3.0 mL of butyl acetate was added under nitrogen protection at a drop rate of about 2 drops / second. After stirring evenly, the temperature was slowly raised to 40°C, stirred for 12 min, and then raised to 80°C. After reacting for 2.5 h, the theoretical value was reached to obtain the prepolymer. The reaction was stopped and sealed for storage at low temperature.
[0060] (2) Preparation of coating: Add 5.0 mL of butyl acetate to the above prepolymer and preheat to 30°C to obtain component A. Heat and dissolve 6.07 g of 3,3'-dichloro-4,4'-diaminodiphenylmethane and 0.52 g of trimethylolpropane in a mixed solution of 8.0 mL of butyl acetate and 0.5 mL of N', N-dimethylformamide as component B. Add component B to component A, stir evenly, and react at a temperature gradient within 30~70°C: slowly heat to 30~40°C and keep warm for 10 min; slowly heat to 40~48°C and keep warm for 20 min; slowly heat to 48~70°C and keep warm for 15 min. After the reaction reaches the theoretical value of the -NCO mass fraction, stop the reaction, add a defoamer, and mix evenly to obtain a polyurethane coating.
[0061] (3) Application of coating: First, the carbon steel surface is sandblasted to remove surface dirt, rust, etc., and the rust removal level reaches Sa 2.5. Then, the polyurethane coating with a diluted solid content of 86% is applied to the carbon steel surface by brushing. The application time is 0.5 h and the thickness is about 2 mm.
[0062] (4) Curing of coating: Place the carbon steel with polyurethane coating on the surface in an atmospheric environment at room temperature of 19-35°C for 7 days to complete moisture curing.
[0063] (5) Cavitation resistance of the coating: Under the aforementioned accelerated cavitation test conditions, the cumulative mass loss of the coating was 0.4 mg after cavitation for 80 h.
[0064] Example 3
[0065] (1) Preparation of -NCO-terminated prepolymer: Add 51.15 g of polytetrahydrofuran ether diol (Mn=2000) into a three-necked flask, preheat to 30°C, and then add 10.00 g of toluene diisocyanate dissolved in 5.0 mL of butyl acetate under nitrogen protection at a drop rate of about 2 drops / second. After stirring evenly, slowly heat to 40°C, stir for 8 min, and then heat to 80°C. After reacting for 2.5 h, the theoretical value is reached to obtain the prepolymer, stop the reaction, and store in a sealed container at low temperature.
[0066] (2) Preparation of coating: Add 5.0 mL of butyl acetate to the above prepolymer and preheat to 30°C to obtain component A. Heat 5.31 g of 3,3'-dichloro-4,4'-diaminodiphenylmethane and 0.78 g of trimethylolpropane and dissolve them in a mixed solution of 6.5 mL of butyl acetate and 0.5 mL of N',N-dimethylformamide to obtain component B. Add component B to component A, stir evenly, and react at a temperature gradient within 30~70°C: slowly heat to 30~40°C and keep warm for 15 minutes; slowly heat to 40~48°C and keep warm for 15 minutes; slowly heat to 48~70°C and keep warm for 15 minutes. After the reaction reaches the theoretical value of the -NCO mass fraction, stop the reaction, add a defoamer, and mix evenly to obtain a polyurethane coating.
[0067] (3) Application of coating: First, the surface of nickel-aluminum bronze is sandblasted to remove surface dirt, rust, etc., and the rust removal level reaches Sa 2.5. Then, the diluted polyurethane coating with a solid content of 60% is applied to the surface of the nickel-aluminum bronze substrate by scraping. The application time is 1.5 hours and the thickness is about 2 mm.
[0068] (4) Curing of coating: Place the nickel-aluminum-bronze substrate coated with polyurethane coating in an atmospheric environment at room temperature of 13-28°C for 7 days to complete moisture curing.
[0069] (5) Cavitation resistance of the coating: Under the aforementioned accelerated cavitation test conditions, the cumulative mass loss of the coating was 0.6 mg after cavitation for 80 h.
[0070] Comparative Example 1
[0071] (1) Preparation of -NCO-terminated prepolymer: Add 51.15 g of polytetrahydrofuran ether diol (Mn=2000) into a three-necked flask, preheat to 30°C, and then add 10.00 g of toluene diisocyanate dissolved in 5.0 mL of ethyl acetate (the type of solvent is not within the scope of protection of the claims) under nitrogen protection, with a drop rate of about 2 drops / second. After stirring evenly, slowly heat to 40°C, stir for 10 min, and then heat to 80°C. After reacting for 2.5 h until the theoretical value is reached, the prepolymer is obtained, the reaction is stopped, and the mixture is sealed and stored at low temperature.
[0072] (2) Preparation of coating: Add 5.0 mL of ethyl acetate to the above prepolymer and preheat to 30°C to obtain component A. Heat and dissolve 4.56 g of 3,3'-dichloro-4,4'-diaminodiphenylmethane and 1.04 g of trimethylolpropane in a mixed solution of 6.5 mL of ethyl acetate and 0.5 mL of N',N-dimethylformamide as component B. Add component B to component A, stir evenly, and react at a temperature gradient within 30~70°C: slowly heat to 30~40°C and keep warm for 10 min; slowly heat to 40~48°C and keep warm for 20 min; slowly heat to 48~70°C and keep warm for 10 min. After the reaction reaches the theoretical value of the -NCO mass fraction, stop the reaction, add a defoamer, and mix evenly to obtain a polyurethane coating.
[0073] (3) Application of coating: First, the stainless steel surface is sandblasted to remove surface dirt, rust, etc., and the rust removal level reaches Sa 2.5. Then, the polyurethane coating with a diluted solid content of 85% is applied to the surface of the stainless steel substrate by brushing. The application time is 1.5 h and the thickness is about 2 mm.
[0074] (4) Curing of coating: Place the stainless steel substrate coated with polyurethane coating in an atmospheric environment at room temperature of 15-25°C for 7 days to complete moisture curing.
[0075] (5) Cavitation resistance of the coating: Under the aforementioned accelerated cavitation test conditions, the cumulative mass loss of the coating was 6.9 mg after cavitation for 80 h.
[0076] Comparative Example 2
[0077] (1) Preparation of -NCO-terminated prepolymer 42.0 g of polytetrahydrofuran ether diol (Mn=1000) (the molecular weight of the polyol is not within the scope of the claims) was added to a three-necked flask, preheated to 30°C, and 28.00 g of isophorone diisocyanate (the type of polyisocyanate is not within the scope of the claims) dissolved in 5.0 mL of ethyl acetate (the type of solvent is not within the scope of the claims) was added under nitrogen protection at a drop rate of about 2 drops / second. After stirring evenly, the temperature was slowly raised to 40°C, stirred for 10 min, and then raised to 80°C. After reacting for 3 h, the theoretical value was reached to obtain a prepolymer, the reaction was stopped, and the mixture was sealed and stored at low temperature.
[0078] (2) Preparation of coating: Add 7.0 mL of ethyl acetate to the above prepolymer and preheat to 30°C as component A. Heat component A to 80°C, add 3.50 g of 1,4-butanediol (the type of chain extender is not within the scope specified in the invention claims) and 3.50 g of trimethylolpropane, react for about 60 minutes until the -NCO mass fraction reaches the theoretical value, stop the reaction, dissolve 2 μL of CUCAT-HA02 catalyst and small molecule additives such as defoaming agent in 6 mL of ethyl acetate, add to the solution, mix well, and obtain a polyurethane coating.
[0079] (3) Application of coating: First, the carbon steel surface is sandblasted to remove dirt, rust, etc. on the surface, and the rust removal level reaches Sa 2.5. Then, the polyurethane coating with a diluted solid content of 90% is applied to the carbon steel surface by brushing. The application time is 0.5 h and the thickness is about 2 mm.
[0080] (4) Curing of coating: Place the carbon steel with polyurethane coating on the surface in an atmospheric environment at room temperature of 19-35°C for 7 days to complete moisture curing.
[0081] (5) Cavitation resistance of the coating: Under the aforementioned accelerated cavitation test conditions, the cumulative mass loss of the coating was 9.8 mg after cavitation for 30 h.
[0082] Comparative Example 3
[0083] The comparative example sample was synthesized with reference to step A of CN 103012736.
[0084] (1) Preparation of -NCO-terminated prepolymer: 40.46 g of preheated and dehydrated polytetramethylene ether diol (Mn=2000) was added to a three-necked flask, preheated to 30°C, and 10.00 g of toluene diisocyanate was added and stirred rapidly. After the temperature stabilized, the temperature was slowly raised and controlled to be 80-85°C. After the reaction reached the theoretical value after 3 h, the prepolymer was obtained. The reaction was stopped, vacuum degassed for 0.5 h, and then sealed for storage.
[0085] (2) Preparation of sample: Take 20.00 g of prepolymer, add 3 drops of DBTDL catalyst and stir evenly, add 7.12 g of 3,3'-dichloro-4,4'-diaminodiphenylmethane and 0.261 g of trimethylolpropane which are melted at high temperature, stir evenly and pour into the mold. After the gel phenomenon appears, close the mold immediately, and react and mold at 10 MPa pressure and 120℃ for 1 h; the demolded test piece is kept at a constant temperature in an oven at 100℃ for 10 h, taken out and left for 7 days, and cut for testing.
[0086] (3) Curing of coating: First, the surface of the substrate is sandblasted to remove dirt, rust, etc. on the surface, and the rust removal level reaches Sa 2.5. The polyurethane coating completely covering the carbon steel surface is prepared using the same method as the sample preparation.
[0087] (4) Cavitation resistance of the coating: Under the aforementioned accelerated cavitation test conditions, the cumulative mass loss of the coating was 9.5 mg after 6 h of cavitation.
[0088] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principle of the present invention shall be equivalent replacement modes and shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a room temperature cured high-toughness cavitation-resistant polyurethane coating, comprising the following process steps: (1) Preparation of -NCO-terminated prepolymer: Add aromatic polyisocyanate dissolved in butyl acetate to the preheated polyol, and adopt a two-stage temperature control method to react. First, slowly heat to 40°C and stir for 5-20 minutes, then continue to heat to 75-80°C and stir for 2-3 hours to obtain the prepolymer, which is then sealed and stored at low temperature. in, The aromatic polyisocyanate is one or more of toluene diisocyanate and diphenylmethane-4,4'-diisocyanate; the polyol is polytetramethylene ether diol with a molecular weight of 2000-3000; the molar ratio of -NCO in the aromatic polyisocyanate to the hydroxyl group in the polyol is 2.4-2.1:1; (2) Preparation of coating: Add butyl acetate to the prepolymer and preheat to 25-35°C to prepare component A; preheat and dissolve a triol crosslinking agent and a chlorine-containing aromatic amine small molecule chain extender with a solvent to prepare component B; add component B to component A, mix well, react at a temperature gradient of 30-70°C for 30-70 minutes, then add a small molecule additive and mix well to obtain a polyurethane coating; The triol crosslinking agent is selected from one or more of trimethylolpropane and trimethylolethane; the chlorine-containing aromatic amine small molecule chain extender is selected from one or more of 3,3'-dichloro-4,4'-diaminodiphenylmethane and 4,4'-methylenebis(3-chloro-2,6-diethylaniline); the total molar ratio of the isocyanate group of the prepolymer in component A to the hydroxyl group and amino group in component B is 1.03-1.10:1; The temperature gradient reaction process is: slowly increase the temperature to 30-40°C, keep warm for 5-15 min; slowly increase the temperature to 40-48°C, keep warm for 5-25 min; slowly increase the temperature to 48-70°C, keep warm for 5-30 min; (3) Application of coating: First, sandblast the surface of the metal substrate to remove dirt and rust on the surface, and make the rust removal level reach at least Sa 2.
5. Then, apply the diluted polyurethane coating to the surface of the substrate by brushing, scraping, dipping, rolling or spraying, with a thickness of 1~3 mm. (4) Curing of coating: Place the substrate coated with polyurethane coating in an atmospheric environment at room temperature for 5 to 10 days to complete moisture curing.
2. The method for preparing a room temperature curing high-toughness cavitation-resistant polyurethane coating as claimed in claim 1, characterized in that: In step (3), the solid content of the diluted polyurethane coating is ≥20%; in step (4), the room temperature curing temperature range is 10~40°C.
3. A high-toughness, cavitation-resistant polyurethane coating prepared by the method of any one of claims 1 to 2.