A high current efficiency multi-component aluminum alloy sacrificial anode and preparation method thereof

By adding Zn, Mg, In, Sn, Bi elements to the aluminum alloy sacrificial anode and performing high-frequency induction smelting and solid solution aging treatment, a stable MgZn2 phase and low temperature communion are formed, and the existing aluminum alloy sacrificial anode is solved. The shortcomings in high current efficiency and long-term discharge stability have achieved efficient current efficiency and the effect of easy fall off of corrosion products, and are suitable for corrosion protection in seawater environments.

CN118166360BActive Publication Date: 2024-11-05CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410483936.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-22
Publication Date
2024-11-05
Estimated Expiration
2044-04-22

AI Technical Summary

Technical Problem

The existing aluminum alloy sacrificial anodes have shortcomings in terms of high current efficiency and long-term discharge stability, especially in seawater environments where current efficiency is reduced and corrosion products are not easily shed.

Method used

Using a high-current efficiency multi-aluminum alloy sacrificial anode, containing Zn, Mg, In, Sn, Bi elements, through high-frequency induction smelting and solid solution aging treatment, a stable MgZn2 phase and low-temperature communion are formed, which improves the activation ability of the anode and Electrochemical properties.

Benefits of technology

It achieves high current efficiency (up to 98.6%) and easy falloff of corrosion products, uniform discharge dissolution, and large actual capacity. It is suitable for corrosion protection of steel structures in seawater environments, reducing self-corrosion rate and pollution risk.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118166360B_ABST
    Figure CN118166360B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of metal corrosion and protective materials, and in particular to a high current efficiency multi-component aluminum alloy sacrificial anode and a preparation method thereof. The high current efficiency multi-component aluminum alloy sacrificial anode comprises the following components by mass percentage: Zn 2.5% to 5.5%, In 0.01% to 0.08%, Mg 1% to 2%, Sn 0.05% to 0.3%, Bi 0.03% to 0.3%, and the remainder is Al and impurity elements, wherein Fe≤0.03%, Si≤0.05%, and Cu≤0.001% are impurity elements. The present invention adopts the above technical scheme, and the obtained high current efficiency multi-component aluminum alloy sacrificial anode has the characteristics of easy detachment of corrosion products, uniform discharge dissolution, high current efficiency, large actual capacitance, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal corrosion and protective materials, and in particular to a high current efficiency multi-component aluminum alloy sacrificial anode and a preparation method thereof. Background Art

[0002] Metal corrosion is a common problem in production and life. It not only reduces the service life of metal components, but also poses a safety hazard in serious cases. Therefore, effective anti-corrosion technology is essential to ensure structural safety and extend service life. Sacrificial anode protection is a commonly used economical and effective anti-corrosion method. Its principle is to connect the protected metal with a metal with strong reducing properties to form a primary battery. When the metal with strong reducing properties dissolves, it generates current, thereby inhibiting the dissolution of the protected metal.

[0003] Sacrificial anode materials mainly include magnesium, zinc and aluminum alloys. Aluminum has attracted much attention due to its advantages such as abundant resources, non-toxicity, relatively negative potential and low density. However, the surface of aluminum is easily passivated in air or aqueous solution, which will cause the potential to shift positively and inhibit further dissolution of the anode, making the protective effect ineffective. Therefore, other alloying elements need to be introduced to destroy the passivation film so that it can continue to dissolve and play the role of the sacrificial anode. Alloying elements such as Zn, Mg, In, and Sn are widely used in aluminum sacrificial anodes. Among them, the Zn element can make the aluminum anode composition uniform, easy to alloy, make the corrosion products easy to fall off, and improve the corrosion resistance of aluminum alloys. Mg, In, Sn, and Bi elements are important activation elements that can destroy the surface passivation film, improve the activation ability of the anode, and make the anode continue to dissolve.

[0004] At present, the commonly used aluminum alloy sacrificial anode systems include aluminum-zinc-mercury (Al-Zn-Hg) system, aluminum-zinc-indium (Al-Zn-In) system, aluminum-zinc-cadmium (Al-Zn-Cd) system, aluminum-zinc-bismuth (Al-Zn-Bi) system, etc. Although these alloy systems have made certain progress in improving current efficiency, there are still some shortcomings. For example, the use of Al-Zn-Hg and Al-Zn-Cd anodes is restricted due to their environmental pollution; Al-Zn-In anodes may have problems such as positive potential shift, uneven surface dissolution and reduced current efficiency after long-term use.

[0005] Patent CN102212829A discloses a high-capacity aluminum alloy sacrificial anode and a preparation method thereof. The aluminum alloy sacrificial anode is composed of aluminum, zinc, indium, tin and magnesium, and is calculated by weight as 94-98 parts of aluminum, 3-5 parts of zinc, 0.04-0.06 parts of indium, 0.06-0.09 parts of tin, and 0.5-1.5 parts of magnesium. The current efficiency of the alloy can only reach 90% at most. Patent CN104060280A discloses an aluminum alloy sacrificial anode with high current efficiency suitable for deep-sea environments. The sacrificial anode is based on aluminum, and zinc, indium, tin, magnesium, and titanium alloy elements are added. The specific composition ratio is (wt%): zinc 4.0-6.0%, indium 0.020-0.030%, tin 0.05-0.10%, magnesium 0.5-1.0%, titanium 0.05-1.0%, wherein the impurities iron <0.050%, copper <0.010%, and the balance is aluminum. The alloy prepared by vacuum smelting has a current efficiency of up to 95.29%, but there are problems of uneven dissolution and corrosion products not falling off during long-term discharge, which leads to a drop in voltage and a decrease in current efficiency. Summary of the invention

[0006] The purpose of the present invention is to provide a high current efficiency multi-component aluminum alloy sacrificial anode and a preparation method thereof. The obtained high current efficiency multi-component aluminum alloy sacrificial anode has the characteristics of easy shedding of corrosion products, uniform discharge dissolution, high current efficiency, large actual capacitance, etc., which solves the above-mentioned technical problems.

[0007] To achieve the above object, the present invention provides a high current efficiency multi-component aluminum alloy sacrificial anode, which comprises the following components by mass percentage: Zn

[0008] 2.5%~5.5%, In 0.01%~0.08%, Mg 1%~2%, Sn 0.05%~0.3%, Bi 0.03%~0.3%, the balance is Al and impurity elements, among which Fe≤0.03%, Si≤0.05%, Cu≤0.001%.

[0009] Preferably, the mass percentage of In is 0.01% to 0.03%. The present invention controls In within the above range, which can effectively reduce the electrode potential of the alloy, promote active dissolution of the anode surface, and avoid the increase in self-corrosion rate due to excessive In content.

[0010] Preferably, the mass percentage of Mg is 1.0% to 1.8%. The present invention controls Mg within the above range, Mg can form a stable compound with Zn, and reduce the adverse effects of impurity elements, while improving the corrosion resistance of the anode.

[0011] Preferably, the mass percentage of Sn is 0.10% to 0.25%. The present invention controls Sn within the above range, and Sn can form a solid solution in the aluminum alloy to destroy the passivation film on the aluminum surface, while avoiding the intergranular corrosion problem caused by excessive Sn content.

[0012] Preferably, the mass percentage of Bi is 0.05% to 0.25%. In the present invention, Bi is controlled within the above range, and Bi can shift the electrode potential of the aluminum anode substrate negatively, thereby improving the electrochemical performance of the alloy.

[0013] Preferably, the actual capacity of the high current efficiency multi-component aluminum alloy sacrificial anode is 2626.0 to 2815.9 Ah·kg -1 , the current efficiency is 92.1% to 98.6%, and the corrosion current density is 3.30μA·cm -2 ~8.98μA·cm -2 .

[0014] The above-mentioned method for preparing a high current efficiency multi-component aluminum alloy sacrificial anode comprises the following steps:

[0015] S1 uses pure aluminum, pure zinc, pure magnesium, pure indium, pure tin and pure bismuth as raw materials, and is prepared according to the mass percentages described in claim 1;

[0016] S2 uses a high-frequency induction melting furnace for melting

[0017] Add pure aluminum, heat the smelting furnace to 780-850°C, sprinkle a covering agent during the smelting process, add pure zinc, pure indium, pure tin and pure bismuth for smelting after the pure aluminum is completely melted, stir evenly with a graphite rod after melting, let it stand for 5-10 minutes, add a refining agent for degassing, let it stand for another 5-10 minutes, remove the slag, pour it into an iron mold preheated to 400-450°C, and obtain a cast alloy after cooling;

[0018] S3: Solution aging treatment of cast alloy

[0019] Solution treatment is to put the cast alloy into a furnace at room temperature, heat it to 420-500℃ at 10-20℃ / min, keep it at that temperature for 2-8h, and then take it out and cool it with water;

[0020] The aging treatment is to place the solution treated alloy into an aging furnace preheated to 120-200°C, keep it warm for 8-16 hours, and then take it out for air cooling.

[0021] Preferably, the pure aluminum, pure zinc and pure magnesium in S1 are pickled before being prepared to remove surface oil and scale, thereby ensuring the purity of the raw materials and avoiding smelting defects such as inclusions caused by metal surface dirt.

[0022] Preferably, the refining agent and covering agent in S2 are placed in an oven before use and dried at 100-130° C. for 60-90 min to remove moisture and volatile impurities in the refining agent and covering agent, avoid sputtering caused by contact of molten metal with water vapor during high-temperature smelting, and reduce gas inclusions that may be generated during the smelting process.

[0023] Preferably, pure zinc, pure magnesium, pure indium, pure tin and pure bismuth in S2 are wrapped with aluminum foil before being added to the smelting furnace, placed in an oven, and dried at 100-130°C for 60-90 minutes. The aluminum foil wrapping can effectively prevent the oxidation of the metal during the high-temperature smelting process, maintain its purity and activity, and make the pure metal easy to operate and transfer. After drying, metal sputtering caused by water vapor contact is avoided, thereby ensuring the safety and stability of the smelting process.

[0024] Mechanism of the present invention:

[0025] The aluminum alloy anode prepared in the present invention is simultaneously alloyed with Zn, Mg, In, Sn, and Bi, wherein the Zn element is formed by forming ZnAl 2 O 4 Destroy the passivation layer and form MgZn with Mg 2 Phase, MgZn after solution aging 2 The phase is evenly distributed on the aluminum alloy matrix (α-Al matrix), promoting the activation and dissolution of the anode alloy. At the same time, Zn and Sn can increase the hydrogen evolution potential and reduce the hydrogen evolution corrosion of the anode. As an activation element, In can significantly reduce the electrode potential of the aluminum alloy anode, making it easier to dissolve. In, Sn, and Bi elements can form a low-temperature eutectic body, making the aluminum surface passivation film microporous and improving the utilization rate of the aluminum anode. In addition, Bi has a large atomic radius. When it is dissolved in the aluminum matrix, it can act as a lattice expander, which helps to increase the solid solubility of activation elements such as In and further enhance the activation ability of the aluminum anode alloy. The interaction of these alloying elements not only reduces the self-corrosion rate of the aluminum alloy anode material, but also effectively improves the electrochemical activity of the sacrificial anode. At the same time, the corrosion products produced are non-toxic and harmless and will not pollute the marine environment.

[0026] Beneficial effects of the present invention:

[0027] (1) The high current efficiency multi-element aluminum alloy sacrificial anode provided by the present invention has a low self-corrosion rate and a high electrochemical activity. The corrosion products produced are non-toxic and harmless and will not pollute the marine environment. It has excellent performance in a seawater environment, a current efficiency of up to 98.6%, an actual capacity of up to 2815.9Ah / kg, and a uniform dissolution morphology, and is suitable for corrosion protection of steel structures in a seawater environment.

[0028] (2) The present invention provides a method for preparing a high current efficiency multi-element aluminum alloy sacrificial anode. By adopting a heat treatment process that combines solid solution treatment with aging treatment, the segregation of alloying elements can be effectively reduced, and the heterogeneity of the microstructure can be improved to obtain a uniform matrix. At the same time, the amount and morphology of the second phase can be adjusted to obtain a second phase with a moderate amount and uniform size, thereby optimizing the alloy microstructure. This not only promotes the uniform dissolution of the anode, but also significantly improves the current efficiency, while reducing the corrosion rate, thereby ultimately obtaining a sacrificial anode with excellent comprehensive performance.

[0029] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is the SEM image of Example 1 of the present invention;

[0031] Figure 2 is the X-ray diffraction spectrum of Examples 1-4 of the present invention;

[0032] Figure 3 1 is a polarization curve diagram of embodiments 1 to 4 of the present invention;

[0033] Figure 4 The surface dissolution morphology diagrams of Examples 1-4 of the present invention after the discharge test. DETAILED DESCRIPTION

[0034] The present invention is further described below in conjunction with the accompanying drawings and embodiments. Unless otherwise defined, the technical terms or scientific terms used in the present invention should be the common meanings understood by people with ordinary skills in the field to which the present invention belongs. The above-mentioned features or features mentioned in the specific examples mentioned in the present invention can be combined arbitrarily, and these specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0035] Example 1

[0036] The present invention provides a high current efficiency multi-element aluminum alloy sacrificial anode, the components of which are shown in Table 1 by mass percentage, specifically: Zn: 5.03%, Mg: 1.52%, In: 0.012%, Sn: 0.11%, Bi: 0.05%, and the remainder is Al and a very small amount of impurities.

[0037] The method for preparing the high current efficiency multi-element aluminum alloy sacrificial anode comprises the following steps:

[0038] S1 uses pure aluminum, pure zinc, pure magnesium, pure indium, pure tin and pure bismuth as raw materials and mixes them according to the above mass percentages;

[0039] Pure aluminum, pure zinc and pure magnesium are pickled before mixing to remove surface oil and oxide scale, and then pure zinc, pure magnesium, pure indium, pure tin and pure bismuth are wrapped with aluminum foil, put into an oven, and dried at 120°C for 80 minutes. At the same time, the refining agent and covering agent are put into an oven before use and dried at 120°C for 80 minutes.

[0040] S2 uses a high-frequency induction melting furnace for melting

[0041] Pure aluminum is added and the smelting furnace is heated to 800°C. A covering agent is sprinkled during the smelting process. After the pure aluminum is completely melted, pure zinc, pure indium, pure tin and pure bismuth are added for smelting. After melting, a graphite rod is used to stir evenly. After standing for 5 minutes, a refining agent is added to degas. After standing for another 10 minutes, the slag is removed and poured into an iron mold preheated to 420°C. After cooling, a cast alloy is obtained.

[0042] S3: Solution aging treatment of cast alloy

[0043] Solution treatment is to put the as-cast alloy into a furnace at room temperature, heat it to 450°C at a rate of 10°C / min, keep it at that temperature for 4 hours, and then take it out and cool it with water;

[0044] The aging treatment is to put the alloy that has undergone solid solution treatment into an aging furnace preheated to 180°C, keep it warm for 8 hours, take it out and air cool it to room temperature to obtain an alloy product.

[0045] The alloy product was sampled and tested. The performance of the alloy product is shown in Table 2. The corrosion current density of the alloy product prepared in this embodiment in 3.5wt% NaCl solution is 3.30μA·cm -2 , the open circuit potential is -1.19V, the working potential is -1.07~-1.09V, and the actual capacitance is 2815.9Ah·kg -1 , the current efficiency is 98.6%.

[0046] Example 2

[0047] A high current efficiency multi-element aluminum alloy sacrificial anode, the components of which are shown in Table 1 by mass percentage, specifically: Zn: 4.91%, Mg: 1.56%, In: 0.013%, Sn: 0.15%, Bi: 0.15%, and the balance is Al and a very small amount of impurities.

[0048] The method for preparing the high current efficiency multi-element aluminum alloy sacrificial anode comprises the following steps:

[0049] S1 uses pure aluminum, pure zinc, pure magnesium, pure indium, pure tin and pure bismuth as raw materials, and mixes them according to the above mass percentages; pure aluminum, pure zinc and pure magnesium are pickled before mixing to remove surface oil and oxide scale, and then pure zinc, pure magnesium, pure indium, pure tin and pure bismuth are wrapped with aluminum foil, put into an oven, and dried at 120°C for 80 minutes. At the same time, refining agent and covering agent are put into an oven before use and dried at 120°C for 80 minutes.

[0050] S2 uses a high-frequency induction melting furnace for melting

[0051] Pure aluminum is added and the smelting furnace is heated to 780°C. A covering agent is sprinkled during the smelting process. After the pure aluminum is completely melted, pure zinc, pure indium, pure tin and pure bismuth are added for smelting. After melting, the alloy is evenly stirred with a graphite rod. After standing for 5 minutes, a refining agent is added for degassing. After standing for another 10 minutes, the slag is removed and poured into an iron mold preheated to 420°C. After cooling, a cast alloy is obtained.

[0052] S3: Solution aging treatment of cast alloy

[0053] Solution treatment is to put the as-cast alloy into a furnace at room temperature, heat it to 450°C at a rate of 10°C / min, keep it at that temperature for 4 hours, and then take it out and cool it with water;

[0054] The aging treatment is to put the alloy that has undergone solid solution treatment into an aging furnace preheated to 180°C, keep it warm for 8 hours, take it out and air cool it to room temperature to obtain an alloy product.

[0055] The alloy product was sampled and tested. The performance of the alloy product is shown in Table 2. The corrosion current density of the alloy product prepared in this embodiment in 3.5wt% NaCl solution is 8.98μA·cm -2 , the open circuit potential is -1.13V, the working potential is -1.07~-1.10V, and the actual capacitance is 2782.9Ah·kg -1 , the current efficiency is 97.5%.

[0056] Example 3

[0057] A high current efficiency multi-element aluminum alloy sacrificial anode, the components of which are shown in Table 1 by mass percentage, specifically: Zn: 4.86%, Mg: 1.60%, In: 0.015%, Sn: 0.23%, Bi: 0.24%, and the balance is Al and a very small amount of impurities.

[0058] The method for preparing the high current efficiency multi-element aluminum alloy sacrificial anode comprises the following steps:

[0059] S1 uses pure aluminum, pure zinc, pure magnesium, pure indium, pure tin and pure bismuth as raw materials and mixes them according to the above mass percentages;

[0060] Pure aluminum, pure zinc and pure magnesium are pickled before mixing to remove surface oil and oxide scale, and then pure zinc, pure magnesium, pure indium, pure tin and pure bismuth are wrapped with aluminum foil, put into an oven, and dried at 120°C for 80 minutes. At the same time, the refining agent and covering agent are put into an oven before use and dried at 120°C for 80 minutes.

[0061] S2 uses a high-frequency induction melting furnace for melting

[0062] Pure aluminum is added and the smelting furnace is heated to 780°C. A covering agent is sprinkled during the smelting process. After the pure aluminum is completely melted, pure zinc, pure indium, pure tin and pure bismuth are added for smelting. After melting, a graphite rod is used to stir evenly. After standing for 5 minutes, a refining agent is added to degas. After standing for another 10 minutes, the slag is removed and poured into an iron mold preheated to 400°C. After cooling, a cast alloy is obtained.

[0063] S3: Solution aging treatment of cast alloy

[0064] Solution treatment is to put the as-cast alloy into a furnace at room temperature, heat it to 450°C at a rate of 10°C / min, keep it at that temperature for 4 hours, and then take it out and cool it with water;

[0065] The aging treatment is to put the alloy that has undergone solid solution treatment into an aging furnace preheated to 180°C, keep it warm for 8 hours, take it out and air cool it to room temperature to obtain an alloy product.

[0066] The alloy product was sampled and tested. The performance of the alloy product is shown in Table 2. The corrosion current density of the alloy product prepared in this embodiment in 3.5wt% NaCl solution is 7.57μA·cm -2 , the open circuit potential is -1.13V, the working potential is -1.06~-1.08V, and the actual capacitance is 2626.0Ah·kg -1 , the current efficiency is 92.1%.

[0067] Example 4

[0068] A high current efficiency multi-element aluminum alloy sacrificial anode, the components of which are shown in Table 1 by mass percentage, specifically: Zn: 4.94%, Mg: 1.53%, In: 0.026%, Sn: 0.14%, Bi: 0.16%, and the balance is Al and a very small amount of impurities.

[0069] The method for preparing the high current efficiency multi-element aluminum alloy sacrificial anode comprises the following steps:

[0070] S1 uses pure aluminum, pure zinc, pure magnesium, pure indium, pure tin and pure bismuth as raw materials and mixes them according to the above mass percentages;

[0071] Pure aluminum, pure zinc and pure magnesium are pickled before mixing to remove surface oil and oxide scale, and then pure zinc, pure magnesium, pure indium, pure tin and pure bismuth are wrapped with aluminum foil, put into an oven, and dried at 120°C for 80 minutes. At the same time, the refining agent and covering agent are put into an oven before use and dried at 120°C for 80 minutes.

[0072] S2 uses a high-frequency induction melting furnace for melting

[0073] Pure aluminum is added and the smelting furnace is heated to 780°C. A covering agent is sprinkled during the smelting process. After the pure aluminum is completely melted, pure zinc, pure indium, pure tin and pure bismuth are added for smelting. After melting, a graphite rod is used to stir evenly. After standing for 5 minutes, a refining agent is added to degas. After standing for another 10 minutes, the slag is removed and poured into an iron mold preheated to 400°C. After cooling, a cast alloy is obtained.

[0074] S3: Solution aging treatment of cast alloy

[0075] The solution treatment is as follows: the cast alloy is placed in a furnace at room temperature, the temperature is raised to 450°C at a rate of 10°C / min, the temperature is kept for 4 hours, and the alloy is taken out and water-cooled.

[0076] The aging treatment is to put the alloy that has undergone solid solution treatment into an aging furnace preheated to 180°C, keep it warm for 8 hours, take it out and air cool it to room temperature to obtain an alloy product.

[0077] The alloy product was sampled and tested. The performance of the alloy product is shown in Table 2. The corrosion current density of the alloy product prepared in this embodiment in a 3.5wt% NaCl solution is 6.06μA·cm -2 , the open circuit potential is -1.16V, the working potential is -1.08~-1.10V, and the actual capacitance is 2689.1Ah·kg -1 , the current efficiency is 94.3%.

[0078] The specific compositions of the alloys of Examples 1-4 are shown in Table 1.

[0079] Table 1 Alloy composition of the multi-component aluminum alloy sacrificial anode embodiment

[0080]

[0081] Table 2 Electrochemical properties of multi-component aluminum alloy sacrificial anodes prepared in Examples 1-4

[0082]

[0083]

[0084] Characterization experiments were performed on the multi-component aluminum alloy sacrificial anodes prepared in Examples 1-4

[0085] Figure 1 It is the SEM picture of Example 1 of the present invention, as Figure 1 As shown in the figure, the microstructure of the aluminum alloy sacrificial anode of Example 1 is composed of an α-Al matrix, fine precipitates precipitated after aging, and coarse precipitates at the grain boundaries, wherein the fine precipitates are MgZn 2 Phase, MgZn 2 The phase is evenly distributed on the α-Al matrix, and the coarse precipitated phase is a (Sn, Bi)-rich phase. Because the solid solubility of Sn and Bi in aluminum alloy is small, it mainly exists in the form of precipitated phase. Figure 2 is the X-ray diffraction spectrum of Examples 1-4 of the present invention, such as Figure 2 As shown, the aluminum alloy sacrificial anodes of Examples 1-4 are mainly composed of α-Al matrix phase. Due to the limited detection accuracy of XRD, the phase with a content of less than 3% may not be detected. Figure 3 is the polarization curve diagram of Examples 1-4 of the present invention; Figure 3 As shown, the aluminum alloy sacrificial anodes of Examples 1-4 all have good corrosion resistance, and Example 1 has the best corrosion resistance. Figure 4 This is a surface dissolution morphology diagram after the discharge test of Examples 1-4 of the present invention, such as Figure 4 As shown, the different aluminum alloy sacrificial anodes of Examples 1-4 have uniform dissolution morphology, no obvious corrosion pits, shallow corrosion depth, and corrosion products that are easy to fall off.

[0086] Therefore, the high current efficiency multi-component aluminum alloy sacrificial anode provided by the present invention has corrosion products that are easy to fall off, uniformly dissolve during discharge, and has a low corrosion rate. 2 The phase is evenly distributed on the substrate and, as a cathode activation point, can effectively destroy the surface passivation film, promote the uniform dissolution of the sacrificial anode, avoid local corrosion concentration, reduce the risk of grain shedding, provide more efficient and stable protection for the protected structure, extend the service life of the sacrificial anode, reduce maintenance costs, and reduce the need for maintenance and replacement due to corrosion.

[0087] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A high current efficiency multi-component aluminum alloy sacrificial anode, Features: The high current efficiency multi-element aluminum alloy sacrificial anode includes the following components by mass percentage: Zn 5.03%, In 0.012%, Mg 1.52%, Sn 0.11%, Bi0.05%, and the balance is Al and impurity elements, wherein Fe≤0.03%, Si≤0.05%, and Cu≤0.001%; The high current efficiency multi-component aluminum alloy sacrificial anode is prepared by the following steps: S1 uses pure aluminum, pure zinc, pure magnesium, pure indium, pure tin and pure bismuth as raw materials and mixes them according to mass percentage; S2 uses a high-frequency induction melting furnace for melting Add pure aluminum, heat the smelting furnace to 800°C, sprinkle a covering agent during the smelting process, add pure zinc, pure indium, pure tin and pure bismuth for smelting after the pure aluminum is completely melted, stir evenly with a graphite rod after melting, let it stand for 5 minutes, add a refining agent for degassing, let it stand for 10 minutes, remove the slag, pour it into an iron mold preheated to 420°C, and obtain a cast alloy after cooling; S3: Solution aging treatment of cast alloy Solution treatment is to put the as-cast alloy into a furnace at room temperature, heat it to 450°C at a rate of 10°C / min, keep it at that temperature for 4 hours, and then take it out and cool it with water; The aging treatment is to put the solution treated alloy into an aging furnace preheated to 180°C, keep it at this temperature for 8 hours, and then take it out and air cool it; The actual capacity of the high current efficiency multi-component aluminum alloy sacrificial anode is 2815.9Ah•kg -1 The current efficiency is 98.6%, and the corrosion current density in 3.5wt% NaCl solution is 3.30μA•cm -2 .

2. A high current efficiency multi-component aluminum alloy sacrificial anode according to claim 1, Features: Pure aluminum, pure zinc and pure magnesium in S1 are pickled before mixing to remove surface oil and oxide scale.

3. The high current efficiency multi-component aluminum alloy sacrificial anode according to claim 1, Features: The refining agent and covering agent in S2 were placed in an oven and dried at 120°C for 80 minutes before use.

4. The high current efficiency multi-component aluminum alloy sacrificial anode according to claim 1, Features: The pure zinc, pure magnesium, pure indium, pure tin and pure bismuth in S2 were wrapped with aluminum foil before being added into the smelting furnace, placed in an oven and dried at 120°C for 80 minutes.