Ultrafine hollow glass microspheres and preparation method thereof
Through the melting, water quenching, crushing and dispersing of glass blocks, combined with polyamide polyamine epoxychlorohydrin oligomer and cellulose ether, the problem of excessive particle size of hollow glass microspheres in the prior art is solved, and the problem of excessive particle size of hollow glass microspheres is realized. Efficient preparation of ultrafine particle size hollow glass microspheres with particle size D90≤30 μm reduces cost and improves compressive resistance.
Patent Information
- Application Number
- CN202410291478.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-14
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-03-14
AI Technical Summary
In the prior art, it is difficult to prepare hollow glass microspheres with particle size D90 below 30 μm, and the glass pulverized material is easily bonded together to form large balls during the ball formation process, resulting in high preparation cost.
Through glass block melting, water quenching, crushing treatment, dispersion treatment and hollow spheroidization treatment, polyamide polyamine epoxy chlorohydrin oligomer solution and cellulose ether improve the dispersion of the pulverized material, avoiding agglomeration and bonding. Ultrafine particle size hollow glass microspheres with particle size D90≤30 μm were directly prepared.
Ultrafine particle size hollow glass microspheres with particle size D90≤30 μm are directly prepared without sorting, reducing the preparation cost and improving the dispersion and compressive resistance of the material.
Smart Images

Figure CN118184112B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of materials, and in particular relates to ultra-fine hollow glass microspheres and a preparation method thereof. Background Art
[0002] Hollow glass microspheres are a kind of glass spheres with rarefied gas inside after special processing. The main component is borosilicate. The general particle size is 10-250 μm and the wall thickness is 1-2 μm. Hollow glass microspheres have the characteristics of low density, high compressive strength, high melting point, high resistivity, sound insulation, small thermal conductivity and thermal shrinkage coefficient. They can be widely used in adhesives, plastics, rubber and other matrices to prepare low-density and other functional materials. In some precision parts and ultra-thin parts applications, the particle size of hollow glass microspheres has an important influence on material properties, and fine particle size has certain advantages in material processing and material appearance. At present, the common particle size D90 of hollow glass microspheres is above 40 μm, and the true density is 0.7 g / cm 3 Below, there are very few hollow microspheres with D90 below 30 μm.
[0003] Chinese patent application CN113354291A discloses a method for preparing hollow glass microspheres for high-frequency and high-speed PCBs, comprising: weighing SiO2: 70% to 80%, B2O3: 5% to 10%, Al2O3: 5% to 10%, CaO: 3% to 5%, Na2O: 1% to 5%, P2O5: 0.5% to 2%, in terms of mass percentage, to form a mixture; melting the mixture at 1400°C to 1500°C for 4 to 6 hours When the glass liquid is obtained and water quenched, a glass material is obtained; the glass material is dried and crushed in turn to obtain a glass powder with a particle size ranging from 1 to 10 μm; the glass powder is sent to a flame burner sintering furnace by gas delivery, spheroidized at 1100°C to 1200°C to obtain glass microspheres, rinsed, dried, sorted, and collected to obtain hollow glass microspheres with a particle size of ≤50 μm; the true density of the hollow glass microspheres is 0.43 to 0.46 g / cm 3 And the particle size D90 is less than 35 μm.
[0004] Although hollow glass microspheres with a particle size D90 < 35 μm are obtained in the above patent application, the preparation method mainly involves rinsing and sorting the finished product after spheroidization, which makes the preparation cost of hollow glass microspheres with a particle size D90 < 35 μm relatively high. In addition, hollow glass microspheres with a particle size D90 below 30 μm are difficult to find on the market. Summary of the invention
[0005] In view of this, the main purpose of the present invention is to provide an ultrafine hollow glass microsphere and a preparation method thereof, which mainly solves the problem that glass crushed materials are easily bonded together to form large balls in the existing ball-forming process, so that the ultrafine hollow glass microsphere can be directly prepared after the glass crushed materials are spheroidized without sorting treatment.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing ultrafine hollow glass microspheres, comprising the steps of:
[0008] Glass block melting and water quenching: firstly, the raw materials for preparing hollow glass microspheres are melted to obtain glass blocks, and then the glass blocks are water quenched to obtain water-quenched materials;
[0009] Crushing treatment: ball milling the water-quenched material to obtain a crushed material with a particle size D90≤17 μm;
[0010] Dispersion treatment: the crushed material, polyamide polyamine epichlorohydrin oligomer solution, cellulose ether and deionized water are uniformly mixed to obtain a crushed material dispersion, and then dried to obtain a dispersed material;
[0011] Hollow spheroidization treatment: hollow spheroidization treatment is performed on the dispersed material to obtain ultra-fine hollow glass microspheres.
[0012] The steps of melting, water quenching, crushing and hollow spheroidization of the glass blocks can all be achieved by using existing technologies.
[0013] Specifically, the step of melting and quenching the glass block may include: first placing the raw material for preparing the hollow glass microspheres in a muffle furnace for melting treatment to obtain a glass block, and then placing the glass block in deionized water to quickly cool it down to obtain a water-quenched material; wherein the melting temperature is preferably 1400-1500°C, such as 1400°C, 1450°C, 1500°C, etc.; the melting time is preferably 5-10 h (hours).
[0014] The raw materials for preparing the hollow glass microspheres are a mixture of raw materials used in the prior art for preparing hollow glass microspheres. For example, the raw materials for preparing the hollow glass microspheres may include 60-70 parts by mass of quartz sand, 8-15 parts by mass of calcium carbonate, 10-18 parts by mass of boric acid, 12-20 parts by mass of sodium carbonate, 3-9 parts by mass of aluminum hydroxide, 1-2 parts by mass of barium carbonate, and 1-2 parts by mass of sodium nitrate. The purity of each raw material is as follows: the purity of quartz sand is 95% or more, the purity of calcium carbonate is 97% or more, the purity of sodium carbonate is 97% or more, the purity of boric acid is 99% or more, the purity of aluminum hydroxide is 99% or more, the purity of barium carbonate is 98% or more, and the purity of sodium nitrate is 99% or more.
[0015] The pulverizing step can pulverize the water-quenched material into a powder with a sufficiently small particle size, and obtain a pulverized material with a particle size D90≤17 μm, so as to directly prepare ultrafine hollow glass microspheres. Preferably, the pulverizing step may include: subjecting the water-quenched material to dry ball milling pulverization to obtain a pulverized material with a particle size D90≤16 μm. In the dry ball milling pulverization process, the mass ratio of the water-quenched material to the zirconium beads is preferably 100: 400-500, the dry ball milling rate is preferably 1800-2200 r / min, and the dry ball milling time is preferably 1-2 h; the particle size D90 of the pulverized material is further preferably 10-16 μm.
[0016] The step of dispersing treatment is mainly to disperse the crushed material to prevent it from agglomerating during the subsequent hollow spheroidization treatment. Adding polyamide polyamine epichlorohydrin oligomer solution and cellulose ether in the step of dispersing treatment is beneficial to improving the dispersibility of glassy crushed material. The main reason is that: polyamide polyamine epichlorohydrin oligomer has a suitably small molecular weight, and it contains a highly polar amide bond that is easily adsorbed on the particle surface in the crushed material. At the same time, it has cations, so that the cations are evenly dispersed on the particle surface, and the particles are in a state of mutual repulsion, thereby improving the dispersibility of the crushed material; and cellulose ether acts as a suspending agent, which can cause the crushed material to suspend in the aqueous solution and promote the dispersion effect. Therefore, polyamide polyamine epichlorohydrin oligomer and cellulose ether can make the dispersion system more uniform and more stable, thereby improving the dispersibility between glass powders, so that the prepared dispersion has good dispersibility.
[0017] Preferably, the polyamide polyamine epichlorohydrin oligomer solution is mainly prepared by the following method: adipic acid and diethylenetriamine are reacted at a molar ratio of 1.15:1.0 at 185-190°C for 2-3 hours, 900% of the total weight of water is added and stirred evenly, epichlorohydrin with a molar amount of 110% to 115% of diethylenetriamine is added at 60-65°C, and the reaction is continued for 3-3.5 hours to obtain a polyamide polyamine epichlorohydrin oligomer solution.
[0018] In order to further ensure the dispersibility of the dispersed material formed by the crushed material and prevent the dispersed material from agglomerating during the subsequent hollow spheroidization process, the mass ratio of the crushed material, the polyamide polyamine epichlorohydrin oligomer solution, the cellulose ether and the deionized water is preferably 100: 4-7: 0.7-1.2 :350~450, such as 100:4:0.7:350, 100:4:0.7:400, 100:4:0.7:450, 100:5:0.9:400, 100:5:0.9:400, 100:6:0.9:400, 100:6:0.9:450, 100:6:1.2:400, 100:7:1.2:350, 100:7:1.2:400, 100:7:1.2:450, etc.; if polyamide polyamine epichlorohydrin If the amount of the polyamide polyamine epichlorohydrin oligomer solution and the cellulose ether is too large, the organic matter between the powder particles is easy to stick together when drying to obtain the dispersion, resulting in larger particles of the ground powder, affecting the particle size of the prepared hollow glass microspheres; if the amount of the polyamide polyamine epichlorohydrin oligomer solution and the cellulose ether is small, the powder particles are easy to agglomerate in the subsequent drying process, making the particles of the dispersion larger, and the glass crushed materials are easy to stick together to form large balls during the ball forming process, thereby making the particle size of the finally prepared hollow glass microspheres larger.
[0019] The hollow spheroidization step may include: adding the dispersed material into a spheroidization furnace for hollow spheroidization, so as to obtain ultrafine hollow glass microspheres with a particle size D90 ≤ 30 μm; wherein the spheroidization temperature is preferably 1300-1400°C. Preferably, the true density of the ultrafine hollow glass microspheres is 0.58-0.65 g / cm 3 , particle size D90 is 15-25 μm, and the 18000 psi compressive crushing rate is <20%, such as 2.5%, 2.8%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, etc.; more preferably, the 18000 psi compressive crushing rate is ≤15%.
[0020] The present invention also provides ultra-fine hollow glass microspheres with a particle size D90≤30 μm prepared by the preparation method.
[0021] Therefore, the ultrafine hollow glass microspheres provided by the present invention are mainly prepared by crushing and dispersing to obtain a dispersed material with a smaller particle size and good dispersibility. In the hollow spheroidization process, the dispersed material still has good dispersibility and is not easy to agglomerate, so that ultrafine hollow glass microspheres with a particle size D90≤30μm can be directly prepared without sorting.
[0022] In addition, the preparation method of the above-mentioned ultrafine hollow glass microspheres provided by the present invention mainly combines a crushing process and a dispersion process, and adds a polyamide polyamine epichlorohydrin oligomer solution and a cellulose ether as a dispersant during the dispersion process, thereby solving the problem that the powder is easy to agglomerate during the ball forming process and the problem that the glass crushed materials are easy to stick together to form large balls during the ball forming process, and realizes that the ultrafine hollow glass microspheres can be prepared by direct spheroidization without sorting, and the preparation method is simple and easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is an optical microscope photograph of the ultrafine hollow glass microspheres provided by Example 1 of the present invention (magnified 200 times).
[0024] Figure 2 This is an optical microscope photograph of the ultrafine hollow glass microspheres provided by Example 3 of the present invention (magnified 200 times). DETAILED DESCRIPTION
[0025] The technical solution of the present invention is further described in detail below through specific implementation methods.
[0026] Unless otherwise specified, the reagents and materials used in the present invention can be purchased through commercial channels. Among them, the purity of the raw materials in the following embodiments is: the purity of quartz sand is more than 95%, the purity of calcium carbonate is more than 97%, the purity of sodium carbonate is more than 97%, the purity of boric acid is more than 99%, the purity of aluminum hydroxide is more than 99%, the purity of barium carbonate is more than 98%, and the purity of sodium nitrate is more than 99%; the viscosity of the cellulose ether used in the following embodiments and comparative examples is 30,000.
[0027] The polyamide polyamine epichlorohydrin oligomer solution used in the following examples and comparative examples was prepared by the following method: adipic acid and diethylenetriamine were reacted at a molar ratio of 1.15:1.0 at 190° C. for 2 h, 900% of the total weight of water was added and stirred evenly, and then epichlorohydrin (110% of the molar amount of diethylenetriamine) was added at 60° C., and the reaction was continued for 3 h to obtain a polyamide polyamine epichlorohydrin oligomer solution.
[0028] Example 1
[0029] This embodiment provides an ultrafine hollow glass microsphere with a particle size D90 of 21 μm, and the preparation method thereof comprises the following steps:
[0030] 1. Raw material configuration (weight parts)
[0031] Quartz sand 60
[0032] Calcium carbonate 15
[0033] Boric acid 10
[0034] Sodium carbonate 12
[0035] Aluminum hydroxide 9
[0036] Barium carbonate 1
[0037] Sodium nitrate 2
[0038] Preparation of raw materials: Mix the above raw materials evenly according to the proportion to obtain a raw material mixture;
[0039] 2. Glass block melting and water quenching
[0040] First, the raw material mixture prepared in step 1 is placed in a furnace at 1460° C. and melted for 10 h to obtain a glass block; then the glass block is placed in deionized water to rapidly cool it down to form a water-quenched material;
[0041] 3. Crushing
[0042] The water-quenched material obtained in step 2 and zirconium beads were put into a ball mill at a mass ratio of 100:400, and dry ball milled at a speed of 1800 r / min for 2 h to prepare a crushed material with a raw material particle size D90 of 14 μm;
[0043] 4. Distributed Processing
[0044] The crushed material in step 3, the polyamide polyamine epichlorohydrin oligomer solution, the cellulose ether and the deionized water are evenly dispersed in a mass ratio of 100:4:1.2:350, and then filtered, dehydrated and dried to obtain a dispersed material;
[0045] 5. Hollow spheroidization treatment
[0046] The dispersed material was added into a spheroidizing furnace and spheronized at 1400°C to obtain hollow glass microspheres with ultra-fine particle size. The optical microscope photo is shown in FIG. Figure 1 shown.
[0047] Example 2
[0048] The present embodiment provides an ultrafine hollow glass microsphere with a particle size D90 of 23 μm. The preparation method of the ultrafine hollow glass microsphere is basically the same as the preparation method of the ultrafine hollow glass microsphere provided in Example 1, with the main difference being that: the crushed material in step “four, dispersion” of the present embodiment: polyamide polyamine epichlorohydrin oligomer solution: cellulose ether: deionized water are in a mass ratio of 100:7:1.2:350, and the other steps and related parameters are the same.
[0049] Example 3
[0050] This embodiment provides an ultrafine hollow glass microsphere with a particle size D90 of 18 μm, and the optical microscope photo is as follows: Figure 2 As shown, the preparation method thereof comprises the following steps:
[0051] 1. Raw material configuration (weight parts)
[0052] Quartz sand 70
[0053] Calcium carbonate 8
[0054] Boric acid 18
[0055] Sodium carbonate 16
[0056] Aluminum hydroxide 6
[0057] Barium carbonate 1.2
[0058] Sodium nitrate 1
[0059] Preparation of raw materials: Mix the above raw materials evenly according to the proportion to obtain a raw material mixture;
[0060] 2. Glass block melting and water quenching
[0061] First, the raw material mixture prepared in step 1 is placed in a furnace at 1400° C. for 8 h to obtain a glass block; then the glass block is placed in deionized water to rapidly cool it down to form a water-quenched material;
[0062] 3. Crushing
[0063] The water-quenched material obtained in step 2 and zirconium beads were put into a ball mill at a mass ratio of 100:500, and dry ball milled at a speed of 2200 r / min for 1.5 h to prepare a crushed material with a raw material particle size D90 of 12 μm;
[0064] 4. Distributed Processing
[0065] The crushed material in step 3, the polyamide polyamine epichlorohydrin oligomer solution, the cellulose ether and the deionized water are evenly dispersed in a mass ratio of 100:7:0.7:450, and then filtered, dehydrated and dried to obtain a dispersed material;
[0066] 5. Hollow spheroidization treatment
[0067] The dispersed material is added into a spheroidizing furnace and spheronized at 1360° C. to obtain hollow glass microspheres with ultra-fine particle size.
[0068] Example 4
[0069] This embodiment provides an ultrafine hollow glass microsphere with a particle size D90 of 25 μm, and the preparation method thereof comprises the following steps:
[0070] 1. Raw material configuration (weight parts)
[0071] Quartz sand 68
[0072] Calcium carbonate 12
[0073] Boric acid 4
[0074] Sodium carbonate 20
[0075] Aluminum hydroxide 3
[0076] Barium carbonate 2
[0077] Sodium nitrate 1.5
[0078] Preparation of raw materials: Mix the above raw materials evenly according to the proportion to obtain a raw material mixture;
[0079] 2. Glass block melting and water quenching
[0080] First, the raw material mixture prepared in step 1 is placed in a furnace at 1500° C. for 5 h to obtain a glass block; then the glass block is placed in deionized water to rapidly cool it down to form a water-quenched material;
[0081] 3. Crushing
[0082] The water-quenched material obtained in step 2 and zirconium beads were put into a ball mill at a mass ratio of 100:450, and dry ball milled at a speed of 1900 r / min for 1 h to prepare a crushed material with a raw material particle size D90 of 16 μm;
[0083] 4. Distributed Processing
[0084] The crushed material in step 3, the polyamide polyamine epichlorohydrin oligomer solution, the cellulose ether and the deionized water are dispersed uniformly in a mass ratio of 100:5:0.8:400, and then filtered, dehydrated and dried to obtain a dispersed material.
[0085] 5. Hollow spheroidization treatment
[0086] The crushed material is added into a pelletizing furnace for hollow spheroidization at 1300° C. to obtain hollow glass microspheres with ultra-fine particle size.
[0087] Comparative Example:
[0088] Comparative Example 1 provides a method for preparing hollow glass microspheres, which is basically the same as the method for preparing ultrafine hollow glass microspheres provided in Example 1, except that the step "IV. Dispersion Treatment" is omitted, and the other steps and related parameters are the same;
[0089] Comparative Example 2 provides a method for preparing hollow glass microspheres, which is basically the same as the method for preparing ultrafine hollow glass microspheres provided in Example 1, except that the dry powder ball milling time in the "III. Crushing Processing" step is 0.5 h, and the other steps and related parameters are the same;
[0090] Comparative Example 3 provides a method for preparing hollow glass microspheres, which is basically the same as the method for preparing ultrafine hollow glass microspheres provided in Example 1, except that the polyamide polyamine epichlorohydrin oligomer solution is not added in the "IV. Dispersion Treatment" step, and the other steps and related parameters are the same;
[0091] Comparative Example 4 provides a method for preparing hollow glass microspheres, which is basically the same as the method for preparing ultrafine hollow glass microspheres provided in Example 1, except that the polyamide polyamine epichlorohydrin oligomer solution in the "IV. Dispersion Treatment" step is replaced with a cellulose ether solution with the same solid content, and the other steps and related parameters are the same;
[0092] Comparative Example 5 provides a method for preparing hollow glass microspheres, which is basically the same as the method for preparing ultrafine hollow glass microspheres provided in Example 1, except that cellulose ether is not added in the "IV. Dispersion Treatment" step, and other steps and related parameters are the same.
[0093] The following tests were performed on the hollow glass microspheres prepared in Examples 1 to 4 and Comparative Examples 1 to 5, and the test results are shown in Table 1.
[0094] The compressive strength of the hollow glass microspheres was measured by the gas pressure method (breakage rate at 18,000 psi), and the true density was tested by the gas displacement method. The D90 particle size of the crushed material and the finished product was measured by a laser particle size analyzer.
[0095] Table 1 Test results of relevant parameters of hollow glass microspheres
[0096]
[0097] Table 1 shows that the ultrafine hollow glass microspheres prepared in Examples 1 to 4 have a D90 particle size of less than 30 μm and a true density of 0.58 to 0.65 g / cm 3 , particle size D90 is 15-25 μm, 18000psi compressive crushing rate is <20%, and it has high compressive resistance.
[0098] From the data of Example 1 and Comparative Example 1, it can be seen that the particle size of the hollow glass microspheres prepared without the dispersion treatment of the crushed material is much larger than the particle size of the product prepared by the dispersion treatment. At the same time, combined with the test results of Comparative Examples 3 to 5, it can be seen that the embodiment of the present invention adopts a combination of polyamide polyamine epichlorohydrin oligomer solution and cellulose ether, and the two act synergistically, so that the powder of the crushed material is more evenly dispersed, the dispersed material has better dispersibility, and the powder does not adhere to each other to form large balls during the balling process, so that ultra-fine hollow glass microspheres can be directly obtained without sorting after hollow spheroidization.
[0099] From the data of Example 1 and Comparative Example 2, it can be seen that the pulverization time has a great influence on the particle size of the finished product. Sufficient pulverization time can grind the water-quenched material finer, which is conducive to the preparation of ultrafine particle size hollow glass microsphere finished products.
[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, ordinary technicians in the field should understand that the specific implementation methods of the present invention can still be modified or some technical features can be replaced by equivalents without departing from the spirit of the technical solution of the present invention, which should be included in the scope of the technical solution for protection of the present invention.
Claims
1. A method for preparing ultrafine hollow glass microspheres, comprising the steps of: Glass block melting and water quenching: firstly, the raw materials for preparing hollow glass microspheres are melted to obtain glass blocks, and then the glass blocks are water quenched to obtain water-quenched materials; Crushing treatment: subjecting the water-quenched material to dry ball milling for 1 to 2 h to obtain a crushed material with a particle size D90 ≤ 16 μm; Dispersion treatment: the crushed material, polyamide polyamine epichlorohydrin oligomer solution, cellulose ether and deionized water are uniformly mixed to obtain a crushed material dispersion, and then dried to obtain a dispersion, wherein: The mass ratio of the crushed material, the polyamide polyamine epichlorohydrin oligomer solution, the cellulose ether and the deionized water is 100: 4-7: 0.7-1.2: 350-450; Hollow spheroidization treatment: hollow spheroidization treatment is performed on the dispersed material to obtain ultrafine hollow glass microspheres with a particle size D90≤30μm; The polyamide polyamine epichlorohydrin oligomer solution is prepared by the following method: adipic acid and diethylenetriamine are reacted at a molar ratio of 1.15:1.0 at 185-190°C for 2-3 hours, 900% of the total weight of water is added and stirred evenly, epichlorohydrin with a molar amount of 110% to 115% of diethylenetriamine is added at 60-65°C, and the reaction is continued for 3-3.5 hours to obtain a polyamide polyamine epichlorohydrin oligomer solution.
2. The preparation method according to claim 1, characterized in that: In the dispersion treatment step, the crushed material dispersion is dried by suction filtration and dehydration to obtain the dispersed material.
3. The preparation method according to claim 1 or 2, characterized in that The particle size D90 of the crushed material is 10 to 16 μm.
4. The preparation method according to claim 3, characterized in that During the dry ball milling process, the mass ratio of the water-quenched material to the zirconium beads is 100:400-500.
5. The preparation method according to claim 3, characterized in that The dry ball milling rate is 1800-2200 r / min.
6. The preparation method according to claim 3, characterized in that: The hollow spheroidization treatment step comprises: adding the dispersed material into a spheroidization furnace, and performing hollow spheroidization at 1300-1400° C. to obtain the ultra-fine hollow glass microspheres.
7. The preparation method according to claim 1, characterized in that: The step of melting and quenching the glass block comprises: firstly placing the raw materials for preparing the hollow glass microspheres in a muffle furnace for melting at 1400-1500° C. to obtain a glass block, and then placing the glass block in deionized water to rapidly cool it down to obtain a water-quenched material.
8. The preparation method according to claim 7, characterized in that The melting time is 5 to 10 h.
9. The preparation method according to claim 1 or 2 or 4 or 5 or 6 or 7 or 8, characterized in that: The raw materials for preparing the hollow glass microspheres include, by weight, 60-70 parts of uniformly mixed quartz sand, 8-15 parts of calcium carbonate, 10-18 parts of boric acid, 12-20 parts of sodium carbonate, 3-9 parts of aluminum hydroxide, 1-2 parts of barium carbonate and 1-2 parts of sodium nitrate.
10. The preparation method according to claim 9, characterized in that: The true density of the ultrafine hollow glass microspheres is 0.58-0.65 g / cm 3 , particle size D90 is 15-25μm, and the compressive crushing rate at 18000psi is less than 20%.