A method for improving the ferroelectric properties of ferroelectric ceramics by high pressure sintering

Through high-temperature solid-state reaction method and cold isostatic pressing combined with vacuum and high-pressure sintering, the problems of low density and volatile elements in the traditional sintering process are solved, and the electrical properties and material purity of ferroelectric ceramics are significantly improved, which is in line with energy conservation and emission reduction. requirements.

CN118184342BActive Publication Date: 2024-10-01SOUTHWEAT UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410243132.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-04
Publication Date
2024-10-01
Estimated Expiration
2044-03-04

AI Technical Summary

Technical Problem

The traditional solid-phase sintering process results in ferroelectric ceramics having low density, coarse grains, high energy consumption, and easy generation of impurity phases, which affects their electrical properties. In addition, lead-free ceramics are easy to volatilize during high-temperature sintering, resulting in reduced performance and incompatible The direction of industrial development in energy conservation and emission reduction.

Method used

Ceramic powder is prepared using a high-temperature solid-state reaction method. After molding by cold isostatic pressing, it is evacuated and sintered at high pressure in a hinged six-sided top press. The sintering pressure and heating rate are precisely controlled to achieve densification and electrical domain refinement of the ceramic. chemical, inhibiting the volatilization of volatile elements.

Benefits of technology

It significantly increases the residual polarization strength of ferroelectric ceramics, improves grain uniformity, reduces sintering energy consumption, shortens the preparation cycle, improves material purity, and meets environmentally friendly and efficient preparation requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118184342B_ABST
    Figure CN118184342B_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving the ferroelectric properties of ferroelectric ceramics by high-pressure sintering, comprising: weighing ferroelectric ceramic raw material powder to prepare ceramic powder; pressing the prepared ceramic powder, performing cold isostatic pressing, and obtaining a ceramic body after pressure maintenance; cutting the ceramic body into block samples, placing the ceramic block samples into a sample assembly of a hinged six-sided top press, evacuating, heating, applying pressure and maintaining pressure at the same time; cooling with the furnace, and taking out a sample of ferroelectric ceramics with enhanced performance. The invention significantly improves the residual polarization strength of ferroelectric ceramics, realizes densification of ceramics, improvement of grain uniformity and refinement of electric domains by precisely controlling the sintering pressure, reduces sintering energy consumption, inhibits the volatilization of volatile elements in the composition of lead-free piezoelectric ceramics, improves the purity of materials, induces internal stress by high-pressure sintering, realizes rapid densification in a short time at a relatively low furnace temperature, and effectively shortens the preparation cycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ferroelectric ceramics, and more specifically, relates to a method for improving the ferroelectric properties of ferroelectric ceramics by high-pressure sintering. Background Art

[0002] Ferroelectric ceramics have the characteristics of non-centrosymmetric structure and convertible polarization, and can produce directional polarization under the action of an external electric field. After polarization, ferroelectric ceramics can retain bound charges related to residual polarization (Pr). They not only have piezoelectric properties and can produce charge separation under mechanical stress, but also show good dielectric properties. Therefore, they are a very important electronic material and are widely used in ferroelectric energy storage devices, piezoelectric transducers, pulse power devices, sensors and electronic devices. Among them, the lead oxide content in PZT ceramic raw materials is about 70%. The strong toxicity and high volatility of lead oxide make lead-based ceramics seriously harmful to the ecological environment during preparation and use. Therefore, it is necessary to develop new alternative lead-free ferroelectric ceramics. Among them, NBT ceramics have attracted much attention among lead-free dielectric materials due to their high Curie temperature (Tc~320℃) and high residual polarization strength.

[0003] At present, the modification of NBT-based ceramic systems is mainly achieved through element doping, multi-component system construction, sintering process optimization and other means to obtain excellent electrical properties. However, traditional solid-phase sintering mainly uses a high-temperature furnace to heat the ceramic raw materials, and the powder blank is gradually densified by the heat generated during the sintering process. Although the traditional sintering process is simple, easy to operate and has low equipment requirements, it still has problems such as low density (95%), coarse grain size and high energy consumption during the sintering process. In addition, the components of lead-free piezoelectric ceramics often contain one or more volatile elements, which are easy to volatilize during the long-term high-temperature sintering preparation process, resulting in impurity phases in the piezoelectric ceramics, resulting in reduced performance. In addition, the long-term high-temperature sintering process will cause high energy consumption and high pollution, which is contrary to the current industrial development direction of energy conservation and emission reduction. Therefore, further optimization of the process is needed to improve its ferroelectric properties. Summary of the invention

[0004] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.

[0005] In order to achieve these purposes and other advantages according to the present invention, a method for improving the ferroelectric properties of ferroelectric ceramics by high pressure sintering is provided, comprising the following steps:

[0006] Step 1, weighing ferroelectric ceramic raw material powder, and preparing ceramic powder by high temperature solid phase reaction method;

[0007] Step 2: Use a mold to press the prepared ceramic powder, then put it into an isostatic press to apply a certain pressure for cold isostatic pressing, and obtain a ceramic body after holding the pressure for a certain period of time;

[0008] Step 3: Cut the ceramic body into block samples, place the ceramic block samples into the sample assembly of the hinged six-sided top press, evacuate the sample, heat it to a certain temperature at a certain heating rate, apply pressure and maintain the pressure; then cool it with the furnace, and take out the ferroelectric ceramic with enhanced ferroelectric properties.

[0009] Preferably, in the step 1, the specific method of preparing the ceramic powder by high temperature solid phase reaction method includes:

[0010] S11, putting the ceramic raw material powder into a ball milling jar, using zirconium oxide as grinding balls and anhydrous ethanol as ball milling medium, and ball milling for a certain period of time in a planetary ball mill;

[0011] S12, sieving the ball-milled ceramic slurry and pouring it into a container, drying it in a blast drying oven, then grinding the dried ceramic powder, pressing the ceramic powder into a cylindrical block using a mold, and then pre-calcining to obtain a pre-calcined ceramic powder;

[0012] S13, placing the pre-fired ceramic powder into a ball mill, adding anhydrous ethanol for secondary ball milling, and then drying.

[0013] Preferably, in said S11, the mass ratio of zirconium oxide, ceramic raw material powder and anhydrous ethanol is 1:1.5:0.6; the ball milling speed is 300-400 r / min, and the ball milling time is 12-36 h.

[0014] Preferably, in said S12, the drying temperature in the blast drying oven is 60-100°C, the drying time is 12-36h, the pre-burning temperature is 800-900°C, and the pre-burning time is 2-6h.

[0015] Preferably, the mass ratio of ceramic powder to anhydrous ethanol in S13 is 2.5:1, the secondary ball milling speed is 200-400 r / min, and the secondary ball milling time is 12-24 h.

[0016] Preferably, in the step 2, the pressure applied by the isostatic press is 150-250 MPa, and the holding time is 1-10 min.

[0017] Preferably, in step 3, the vacuum degree of the vacuum pump is 0.5×10 -2 ~1.5×10 -2Pa, the heating rate is 10-30°C / min, the heating temperature is 1200-1300°C, the applied pressure is 1500-4000MPa, and the holding time is 20-60min.

[0018] Preferably, the ferroelectric ceramic raw material powder comprises 52.26 wt % Bi 2 O 3 Powder, 35.85wt% TiO 2 powder and 11.89wt% Na 2 CO 3 powder.

[0019] Preferably, the remanent polarization intensity of the ferroelectric ceramic with enhanced ferroelectric properties is greater than or equal to 32.8 μC / cm 2 .

[0020] The present invention includes at least the following beneficial effects: The present invention innovatively proposes a high-pressure sintering preparation method for lead-free ferroelectric ceramics, which significantly improves the electrical properties of ferroelectric ceramics, including a significant enhancement of residual polarization intensity. By precisely controlling the sintering pressure, the densification of the ceramics, the improvement of grain uniformity and the refinement of the electric domain are achieved, while the sintering energy consumption is reduced, which is in line with the current development direction of industrial energy conservation and emission reduction. The method also successfully inhibits the volatilization of volatile elements in the composition of lead-free piezoelectric ceramics, improves the purity of the material, and at the same time induces internal stress through high-pressure sintering, achieving rapid densification in a short time at a relatively low furnace temperature, effectively shortening the preparation cycle, and providing a feasible way for the preparation of environmentally friendly and efficient ferroelectric ceramics.

[0021] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the SEM image of the NBT ceramic prepared in Example 1 under a sintering pressure of 3000 MPa. DETAILED DESCRIPTION

[0023] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.

[0024] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.

[0025] Example 1

[0026] This embodiment provides a method for improving the ferroelectric properties of ferroelectric ceramics by high pressure sintering, comprising the following steps:

[0027] Step 1: Weigh 52.26wt% Bi 2 O 3 Powder, 35.85wt% TiO 2 powder and 11.89wt% Na 2 CO 3 Powder, the purity is greater than 99.9wt%, NBT ceramics ((Bi 0.5 Na 0.5 )TiO 3 ) powder, specifically including:

[0028] S11, put the raw materials into a ball mill prepared in advance, use zirconium oxide as grinding balls and anhydrous ethanol as grinding medium, and mill them in a planetary ball mill at a speed of 350 r / min for 24 hours;

[0029] S12, the ceramic slurry after ball milling is sieved and poured into a container, and the temperature is still maintained at 80°C for 24 hours in a blast drying oven for drying, and then the powder is ground and pressed into a cylindrical block with a diameter of 30 cm using a mold, and a suitable temperature is selected for pre-sintering. The pre-sintering condition is sintering at 850°C for 4 hours. The purpose of pre-sintering is to make the raw materials in the ceramic fully react to obtain preliminary ceramic powder;

[0030] S13, the calcined powder is ground again, and the obtained powder is placed in a ball mill and anhydrous ethanol is added for secondary ball milling, which needs to be ball milled at a speed of 380r / min for 18h; and then dried;

[0031] Step 2: Use a mold to press the prepared ceramic powder into a disc with a diameter of 30 mm and a thickness of about 1.5 mm, and then put it into an isostatic press to apply a pressure of 200 MPa for cold isostatic pressing. The holding time is set to 5 minutes to obtain a ceramic body with a smooth surface and a certain mechanical strength;

[0032] Step 3: Cut the prepared ceramic body into block samples of 7×7×5 mm, place the body into the sample assembly of the domestic hinged six-sided top press, and evacuate to 10 -2 Pa, start heating to 1250℃ at a rate of 20℃ / min, apply pressure to 3000MPa, and keep warm for 30min. Then cool with the furnace, the ceramic powder fully reacts at the target temperature, and obtains a ceramic sheet with high density and high strength; finally, open the furnace to release the pressure and take out the ceramic sample.

[0033] Example 2

[0034] This embodiment provides a method for improving the ferroelectric properties of ferroelectric ceramics by high-pressure sintering. The difference from Embodiment 1 is that the pressure applied in step three is 1500 MPa, and the rest of the process is the same as that of Embodiment 1.

[0035] Example 3

[0036] This embodiment provides a method for improving the ferroelectric properties of ferroelectric ceramics by high-pressure sintering. The difference from Embodiment 1 is that the pressure applied in step three is 2000 MPa, and the rest of the process is the same as that of Embodiment 1.

[0037] Example 4

[0038] This embodiment provides a method for improving the ferroelectric properties of ferroelectric ceramics by high-pressure sintering. The difference from Embodiment 1 is that the pressure applied in step three is 2500 MPa, and the rest of the process is the same as that of Embodiment 1.

[0039] Example 5

[0040] This embodiment provides a method for improving the ferroelectric properties of ferroelectric ceramics by high-pressure sintering. The difference from Embodiment 1 is that the pressure applied in step three is 3500 MPa, and the rest of the process is the same as that of Embodiment 1.

[0041] Example 6

[0042] This embodiment provides a method for improving the ferroelectric properties of ferroelectric ceramics by high-pressure sintering. The difference from Embodiment 1 is that the pressure applied in step three is 1500 MPa, and the rest of the process is the same as that of Embodiment 1.

[0043] Comparative Example 1

[0044] This embodiment provides a method for improving the ferroelectric properties of ferroelectric ceramics by high-pressure sintering. The difference from Embodiment 1 is that the pressure applied in step three is atmospheric pressure, and the rest of the process is the same as that of Embodiment 1.

[0045] Comparative Example 2

[0046] This embodiment provides a method for improving the ferroelectric properties of ferroelectric ceramics by high-pressure sintering. The difference from Embodiment 1 is that the pressure applied in step three is 500 MPa, and the rest of the process is the same as that of Embodiment 1.

[0047] Comparative Example 3

[0048] This embodiment provides a method for improving the ferroelectric properties of ferroelectric ceramics by high-pressure sintering. The difference from Embodiment 1 is that the pressure applied in step three is 1000 MPa, and the rest of the process is the same as that of Embodiment 1.

[0049] The sintered samples of Examples 1 to 6 and Comparative Examples 1 to 3 were pre-grinded, and the hysteresis loops of the sintered samples were measured using a ferroelectric analyzer. The following table was obtained by measuring the information of the hysteresis loops and the residual polarization intensity of the samples:

[0050] Table 1 Remanent polarization intensity and Curie temperature of NBT ceramics under different pressures

[0051]

[0052]

[0053] It can be seen from the above table that the NBT ceramics sintered in Examples 1 to 6 have greater residual polarization intensity than the NBT ceramics sintered in Comparative Examples 1 to 3, and the Curie temperature does not decrease; among them, the residual polarization intensity of the NBT ceramic sintered in Example 1 under a pressure of 3000 MPa is the largest, reaching 40.7 μC / cm 2 .

[0054] The number of devices and processing scales described here are used to simplify the description of the present invention. Applications, modifications and variations of the present invention will be obvious to those skilled in the art.

[0055] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.

Claims

1. A method for improving the ferroelectric properties of ferroelectric ceramics by high pressure sintering, characterized in that: The following steps are involved: Step 1, weighing ferroelectric ceramic raw material powder, and preparing ceramic powder by high temperature solid phase reaction method; Step 2: Use a mold to press the prepared ceramic powder, then put it into an isostatic press to apply a certain pressure for cold isostatic pressing, and obtain a ceramic body after holding the pressure for a certain period of time; Step 3: Cut the ceramic body into block samples, put the ceramic block samples into the sample assembly of the hinged six-sided top press, evacuate, heat to a certain temperature at a certain heating rate, and apply pressure and maintain the pressure; Then the furnace is cooled and the ferroelectric ceramic with enhanced ferroelectric properties is taken out; In the step 1, the specific method of preparing ceramic powder by high temperature solid phase reaction method includes: S11, putting the ceramic raw material powder into a ball milling jar, using zirconium oxide as grinding balls and anhydrous ethanol as ball milling medium, and ball milling for a certain period of time in a planetary ball mill; S12, sieving the ball-milled ceramic slurry and pouring it into a container, drying it in a blast drying oven, then grinding the dried ceramic powder, pressing the ceramic powder into a cylindrical block using a mold, and then pre-calcining to obtain a pre-calcined ceramic powder; S13, placing the pre-sintered ceramic powder into a ball mill, adding anhydrous ethanol for secondary ball milling, and then drying; In the S11, the mass ratio of zirconium oxide, ceramic raw material powder and anhydrous ethanol is 1:1.5:0.6; the ball milling speed is 300-400 r / min, and the ball milling time is 12-36 h; In S13, the mass ratio of ceramic powder to anhydrous ethanol is 2.5:1, the secondary ball milling speed is 200-400 r / min, and the secondary ball milling time is 12-24 h; In step 3, the vacuum degree of the vacuum pump is 0.5×10 -2 ~1.5×10 -2 Pa, heating rate is 10~30℃ / min, heating temperature is 1200~1300℃, applied pressure is 1500~4000 MPa, and holding time is 20~60 min; The ferroelectric ceramic raw material powder includes 52.26wt% Bi2O3 powder, 35.85wt% TiO2 powder and 11.89wt% Na2CO3 powder; The residual polarization intensity of the ferroelectric ceramic with enhanced ferroelectric performance is greater than or equal to 32.8 μC / cm 2 .

2. The method for improving the ferroelectric properties of ferroelectric ceramics by high pressure sintering as claimed in claim 1, characterized in that: In S12, the drying temperature in the blast drying oven is 60-100°C, the drying time is 12-36 hours, the pre-burning temperature is 800-900°C, and the pre-burning time is 2-6 hours.

3. The method for improving the ferroelectric properties of ferroelectric ceramics by high pressure sintering as claimed in claim 1, characterized in that: In the step 2, the pressure applied by the isostatic press is 150-250 MPa, and the holding time is 1-10 min.