A method for treating waste carbon-carbon composite materials

By grinding the carbon-carbon composite waste into powder and mixing it with specific additives for hot pressing, it is solved by carbonization, densification and purification, and the preparation cycle, high cost and molding of carbon-carbon composite waste recycling is solved. The difficult problem has achieved efficient and stable production of carbon-carbon composite materials.

CN118184381BActive Publication Date: 2024-11-08ZHEJIANG XINGHUI NEW MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410288739.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-13
Publication Date
2024-11-08
Estimated Expiration
2044-03-13

AI Technical Summary

Technical Problem

The problem of recycling and reuse of carbon-carbon composite waste is that the traditional process has a long preparation cycle, high cost, unstable finished product size and low yield.

Method used

The carbon-carbon composite waste is ground into carbon fiber powder, mixed with carbon fiber chopped wire, phenolic resin powder, silicon carbide and liquid phenolic resin, and then carbonized, densified and purified after hot pressing.

Benefits of technology

It improves the recycling efficiency of carbon-carbon composite materials, reduces production costs, shortens production cycles, improves the bending strength and yield of finished products, and solves the problem of difficult molding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118184381B_ABST
    Figure CN118184381B_ABST
Patent Text Reader

Abstract

The present invention provides a method for treating waste carbon-carbon composite materials, comprising the following steps: a) grinding the waste carbon-carbon composite materials to obtain carbon fiber powder; b) mixing the carbon fiber powder obtained in step a) with carbon fiber chopped strands, phenolic resin powder, silicon carbide, and liquid phenolic resin, placing the mixture in a mold for hot pressing, and then sequentially carbonizing, densifying, and purifying to obtain a carbon-carbon composite material. Compared with the prior art, the method for treating waste carbon-carbon composite materials provided by the present invention selects specific raw materials and cooperates with specific process steps to achieve overall good interaction, which can solve the problem of recycling waste carbon-carbon composite materials, is conducive to improving efficiency and saving costs; at the same time, it solves the problem of difficulty in forming special-shaped parts of carbon-carbon composite materials in the preform production stage, and improves the yield; and it can also shorten the production cycle and improve production capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of waste resource utilization, and more specifically, to a method for treating carbon-carbon composite waste. Background Art

[0002] The carbon-carbon composite material industry has developed rapidly in China in recent years. Due to its good mechanical properties and the property of not deforming at high temperatures, it has been widely used in many application scenarios protected by high-temperature inert gases. However, the more application scenarios there are, the more carbon-carbon composite materials are produced, and the more carbon-carbon composite material waste is generated after the material fails. How to solve the recycling and reuse of carbon-carbon composite material waste has become a technical problem that needs to be urgently solved by technicians in this field.

[0003] The traditional process of making special-shaped parts of carbon-carbon composite materials is: carbon fiber raw fibers are cut into short strands → the short strands are combed into a mesh (mesh tire) → the mesh tire + carbon cloth are 2.5D needle-punched into a preform on a mold → the preform is dipped in glue → solidified and shaped → carbonized to remove non-carbon elements → densified to fill the pores inside the carbon-carbon part → high-temperature purification above 2300°C to further remove non-carbon elements.

[0004] However, the traditional process has the following disadvantages: (1) The preform preparation cycle is long, and the preparation process requires fiber chopping, combing the chopped fibers into a web, and needle punching the web into a preform. The preparation cycle of the preform is usually 7 days in total, and the preparation cost is high; (2) During the dipping and curing stage, the fibers soften and are easily deformed after the preform is dipped in the glue, and the size changes greatly after curing, making it difficult to obtain the designed shape, and the defective products reach more than 50%; (3) The densification cycle is long, and the preform density is 0.45g / cm 3 The density of the finished product needs to be 1.4g / cm 3 The huge density difference between the preform and the finished product results in a long densification cycle. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a method for treating carbon-carbon composite waste, which can solve the problem of recycling carbon-carbon composite waste, which is beneficial to improving efficiency and saving costs; at the same time, it solves the problem of difficulty in forming carbon-carbon composite special-shaped parts in the preform production stage, thereby improving the yield; and it can also shorten the production cycle and improve production capacity.

[0006] The present invention provides a method for treating carbon-carbon composite waste, comprising the following steps:

[0007] a) grinding the carbon-carbon composite waste to obtain carbon fiber powder;

[0008] b) mixing the carbon fiber powder obtained in step a) with carbon fiber chopped strands, phenolic resin powder, silicon carbide and liquid phenolic resin, placing the mixture in a mold for hot pressing, and then sequentially carbonizing, densifying and purifying the mixture to obtain a carbon-carbon composite material.

[0009] Preferably, the carbon-carbon composite waste in step a) includes scrapped carbon-carbon composite materials, leftovers and scraps generated during processing, and carbon shreds generated during processing.

[0010] Preferably, the grinding fineness in step a) is 100 mesh to 400 mesh.

[0011] Preferably, the carbon fiber chopped strands in step b) are obtained by crushing carbon fiber waste; the carbon fiber waste includes scraps, webs, and preform scraps generated in the process of weaving carbon fiber cloth.

[0012] Preferably, the length of the crushing process is 10 mm to 100 mm.

[0013] Preferably, in step b), the mass ratio of the carbon fiber powder, carbon fiber chopped strands, phenolic resin powder, silicon carbide and liquid phenolic resin is 1:(8-10):(7-9):(0.5-1.5):(0.5-1.5).

[0014] Preferably, the mixing method in step b) is stirring; the stirring temperature is 10° C. to 40° C., the rotation speed is 60 r / min to 80 r / min, and the time is 20 min to 40 min.

[0015] Preferably, the temperature of the hot pressing molding in step b) is 150° C. to 180° C., the pressure is 5 MPa to 10 MPa, and the time is 3600 s to 7200 s.

[0016] Preferably, the carbonization process in step b) is specifically as follows:

[0017] Treat at 800℃~900℃ for 1h~2h under nitrogen environment protection.

[0018] Preferably, the densification in step b) adopts liquid phase impregnation phenolic resin-carbonization technology, and after impregnation with the resin, it is treated at 800°C to 900°C for 1h to 2h under nitrogen environment protection, and repeated 2 to 4 times; the purification is treated at 2300°C to 2400°C for 1h to 2h under argon environment protection.

[0019] The present invention provides a method for treating waste carbon-carbon composite materials, comprising the following steps: a) grinding the waste carbon-carbon composite materials to obtain carbon fiber powder; b) mixing the carbon fiber powder obtained in step a) with carbon fiber chopped strands, phenolic resin powder, silicon carbide, and liquid phenolic resin, placing the mixture in a mold for hot pressing, and then sequentially carbonizing, densifying, and purifying to obtain a carbon-carbon composite material. Compared with the prior art, the method for treating waste carbon-carbon composite materials provided by the present invention selects specific raw materials and cooperates with specific process steps to achieve overall good interaction, which can solve the problem of recycling waste carbon-carbon composite materials, is conducive to improving efficiency and saving costs; at the same time, it solves the problem of difficulty in forming special-shaped parts of carbon-carbon composite materials in the preform production stage, and improves the yield; and it can also shorten the production cycle and improve production capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The present invention provides a process flow chart of the method for treating carbon-carbon composite waste. DETAILED DESCRIPTION

[0021] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] The present invention provides a method for treating carbon-carbon composite waste, comprising the following steps:

[0023] a) grinding the carbon-carbon composite waste to obtain carbon fiber powder;

[0024] b) mixing the carbon fiber powder obtained in step a) with carbon fiber chopped strands, phenolic resin powder, silicon carbide and liquid phenolic resin, placing the mixture in a mold for hot pressing, and then sequentially carbonizing, densifying and purifying the mixture to obtain a carbon-carbon composite material.

[0025] The present invention first grinds the carbon-carbon composite waste to obtain carbon fiber powder. In the present invention, the carbon-carbon composite waste preferably includes waste carbon-carbon composite materials, scraps generated by processing, scraps and carbon shreds generated during processing; and can be obtained by recycling methods well known to those skilled in the art or purchased from the market.

[0026] In the present invention, the grinding fineness is preferably 100 mesh to 400 mesh.

[0027] After obtaining the carbon fiber powder, the present invention mixes the obtained carbon fiber powder with carbon fiber chopped strands, phenolic resin powder, silicon carbide, and liquid phenolic resin, places the mixture in a mold for hot pressing, and then sequentially carbonizes, densifies, and purifies the mixture to obtain a carbon-carbon composite material.

[0028] In the present invention, the carbon fiber chopped strands are preferably obtained by crushing carbon fiber waste; the carbon fiber waste preferably includes scraps, webs, and preform scraps generated in the process of weaving carbon fiber cloth; they can also be obtained by recycling methods well known to technicians in this field or purchased from the market.

[0029] In the present invention, the length of the crushing process is preferably 10 mm to 100 mm.

[0030] The present invention has no special restrictions on the sources of the phenolic resin powder, silicon carbide and liquid phenolic resin, and commercially available products known to those skilled in the art may be used.

[0031] In the present invention, the mass ratio of the carbon fiber powder, carbon fiber chopped strands, phenolic resin powder, silicon carbide and liquid phenolic resin is preferably 1:(8-10):(7-9):(0.5-1.5):(0.5-1.5), more preferably 1:9:8:1:1.

[0032] In the present invention, the mixing method is preferably stirring, using a stirrer well known to those skilled in the art; the stirring temperature is preferably 10°C to 40°C, more preferably 20°C to 30°C, the rotation speed is preferably 60r / min to 80r / min, and the time is preferably 20min to 40min.

[0033] The mixture obtained after mixing is placed in a mold for hot pressing molding.

[0034] In the present invention, the temperature of the hot pressing molding is preferably 150° C. to 180° C., the pressure is preferably 5 MPa to 10 MPa, and the time is preferably 3600 s to 7200 s.

[0035] The obtained molded body is then successively carbonized, densified and purified to obtain a carbon-carbon composite material product.

[0036] In the present invention, the carbonization process is preferably specifically as follows:

[0037] Treat at 800℃~900℃ for 1h~2h under nitrogen environment protection.

[0038] In the present invention, the densification preferably adopts liquid phase impregnation phenolic resin-carbonization technology, and after impregnation with the resin, the resin is treated at 800℃~900℃ for 1h~2h under nitrogen environment protection, and repeated 2 times to 4 times. The present invention has no special restrictions on the type and source of the resin, and commercial products well known to those skilled in the art can be used; in a preferred embodiment of the present invention, the manufacturer model of the resin is Shengquan-PF9701.

[0039] In the present invention, the purification is preferably carried out under argon environment protection at 2300° C. to 2400° C. for 1 h to 2 h.

[0040] The processing method and raw material formula provided by the present invention, on the basis of solving the recycling of carbon-carbon composite waste (improving efficiency and saving costs), the obtained product can meet the use requirements of carbon-carbon composite materials; and the bending strength of the product is greatly improved; at the same time, the processing method provided by the present invention is easy to form, and the finished product has high dimensional stability, which solves the problem of difficult forming of carbon-carbon composite special-shaped parts in the preform production stage, improves the yield, and can shorten the production cycle and increase production capacity.

[0041] The present invention provides a method for treating waste carbon-carbon composite materials, comprising the following steps: a) grinding the waste carbon-carbon composite materials to obtain carbon fiber powder; b) mixing the carbon fiber powder obtained in step a) with carbon fiber chopped strands, phenolic resin powder, silicon carbide, and liquid phenolic resin, placing the mixture in a mold for hot pressing, and then sequentially carbonizing, densifying, and purifying to obtain a carbon-carbon composite material. Compared with the prior art, the method for treating waste carbon-carbon composite materials provided by the present invention selects specific raw materials and cooperates with specific process steps to achieve overall good interaction, which can solve the problem of recycling waste carbon-carbon composite materials, is conducive to improving efficiency and saving costs; at the same time, it solves the problem of difficulty in forming special-shaped parts of carbon-carbon composite materials in the preform production stage, and improves the yield; and it can also shorten the production cycle and improve production capacity.

[0042] In order to further illustrate the present invention, the following examples are used to provide a detailed description. The carbon-carbon composite waste used in the following examples of the present invention mainly includes scrapped carbon-carbon composite materials, scraps generated by processing, scrapped materials and carbon pulverized dust generated during processing, the carbon fiber waste used mainly includes scraps, mesh tires, and preform scraps generated during the weaving of carbon fiber cloth, the phenolic resin powder used is WL-YP8008 provided by Weilin, the silicon carbide used is 200-300 mesh silicon carbide provided by Guangzhou Metallurgy, and the liquid phenolic resin used is PF9701 provided by Shengquan.

[0043] Example 1

[0044] (1) Grinding carbon-carbon composite waste into carbon fiber powder with a fineness of 200-300 mesh; at the same time, breaking the carbon fiber waste into 50 mm short chopped strands; putting the two into a blender in a certain proportion, and adding a certain amount of phenolic resin powder, silicon carbide and liquid phenolic resin, stirring evenly (room temperature, 80 r / min, 30 min) to obtain a mixture; the mass ratio of the above carbon fiber short filaments, carbon fiber powder, silicon carbide, phenolic resin powder and liquid phenolic resin is 45:5:5:40:5.

[0045] (2) The mixture obtained in step (1) is placed into a mold and hot-pressed (150°C, 5MPa, 3600s). The obtained molded body is placed in a carbonization furnace for carbonization treatment at 800°C for 2h. The carbonized product is successively impregnated with resin and carbonized at 800°C for 2h to achieve the purpose of densification. The densification needs to be repeated 3 times. The densified product is then placed in a purification furnace for high-temperature purification at 2400°C for 1h to obtain a carbon-carbon composite material, thereby realizing the recycling of the carbon-carbon composite material.

[0046] Comparative Example 1

[0047] The treatment method provided in Example 1 is adopted, except that: in step (1), the carbon fiber waste is broken into 50 mm short chopped strands and put into a blender, and a certain amount of phenolic resin powder is added and stirred evenly (room temperature, 80 r / min, 30 min) to obtain a mixture; the mass ratio of the above carbon fiber short strands and phenolic resin powder is 55:45.

[0048] Comparative Example 2

[0049] The treatment method provided in Example 1 is adopted, except that: in step (1), carbon powder is put into a blender, and a certain amount of phenolic resin powder is added, and stirred evenly (room temperature, 80r / min, 30min) to obtain a mixture; the mass ratio of the above carbon powder and phenolic resin powder is 55:45.

[0050] Comparative Example 3

[0051] The treatment method provided in Example 1 is adopted, except that: in step (1), the carbon fiber waste is crushed into 50 mm short chopped strands and carbon powder and put into a blender, and a certain amount of phenolic resin powder is added and stirred evenly (room temperature, 80 r / min, 30 min) to obtain a mixture; the mass ratio of the above-mentioned carbon fiber short strands, carbon powder and phenolic resin powder is 45:10:45.

[0052] Comparative Example 4

[0053] The treatment method provided in Example 1 is adopted, except that: in step (1), the carbon fiber waste is crushed into 50 mm short chopped strands and carbon powder and put into a blender, and a certain amount of phenolic resin powder and silicon carbide are added and stirred evenly (room temperature, 80 r / min, 30 min) to obtain a mixture; the mass ratio of the above-mentioned carbon fiber short strands, carbon powder, silicon carbide and phenolic resin powder is 45:5:5:45.

[0054] Comparative Example 5

[0055] Traditional needle punching process.

[0056] (1) Cut the carbon fiber raw yarn into short chopped strands of 60 mm to 100 mm; then comb the short chopped strands into 50 to 70 g / m 2 , 0.5-1mm thick mesh; then 200-250g / m 2 , 0.4mm thick carbon cloth and mesh tire needle punch compound volume density 0.45 ~ 0.6g / cm 3 , a preform with a thickness of 10 to 15 mm; and then impregnating the preform with liquid phenolic resin, wherein the mass ratio of the preform to the liquid phenolic resin is 45:55.

[0057] (2) The mixture obtained in step (1) is placed in a mold and hot-pressed (150°C, 5MPa, 3600s). The obtained molded body is placed in a carbonization furnace for carbonization treatment at 800°C for 2h. The carbonized product is successively impregnated with resin and carbonized at 800°C for 2h to achieve the purpose of densification. The densification needs to be repeated 4 times. The densified product is then placed in a purification furnace for high-temperature purification at 2400°C for 1h to obtain a carbon-carbon composite material.

[0058] The products of the above-mentioned embodiments and comparative examples were subjected to bending strength test and appearance evaluation. The results are shown in Table 1 below.

[0059] Table 1 Bending strength data and appearance evaluation of products of Examples and Comparative Examples

[0060] Bending strength(MPa) Product Appearance Comparative Example 1 120 Surface pits, roughness, no shape, and pores after processing Comparative Example 2 40 The product cracks, deforms, and has pores after carbonization. Comparative Example 3 140 The product does not crack, does not deform, has a good appearance, and has pores after processing Comparative Example 4 160 The product does not crack, does not deform, has a good appearance, and has pores after processing Example 1 180 The product does not crack, does not deform, has a good appearance, and has no pores after processing Comparative Example 5 120 The product does not crack, does not deform, has a good appearance, and has no pores after processing

[0061] The experimental results show that the treatment method and raw material formula provided by the present invention, on the basis of solving the recycling of carbon-carbon composite waste (improving efficiency and saving costs), the obtained product can meet the use requirements of carbon-carbon composite materials; and the bending strength of the product is improved by (180-120) / 120×100%=50% compared with the product obtained by traditional process.

[0062] At the same time, the processing method provided by the present invention is easy to form, and the finished product has high dimensional stability, which solves the problem of difficult forming of carbon-carbon composite material special-shaped parts in the preform production stage, improves the yield rate, and can increase the yield rate from 50% to 99%, and shortens the production cycle and improves production capacity; see Table 2 below.

[0063] Table 2 Comparison of yield and production cycle

[0064] Technology Preform production cycle (h) Densification + purification cycle (h) Total cycle (h) First yield Comparative Example 5 56 1126 1182 50% Example 1 3 936 939 99%

[0065] Experimental results show that the present invention saves 1182h-939h=243h, or about ten days, in producing a finished product compared with the traditional process, and the production capacity in the preform forming stage is increased by 18.66 times.

[0066] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for treating carbon-carbon composite waste, comprising the following steps: a) grinding carbon-carbon composite waste to obtain carbon fiber powder; b) mixing the carbon fiber powder obtained in step a) with carbon fiber chopped strands, phenolic resin powder, silicon carbide and liquid phenolic resin, placing the mixture in a mold for hot pressing, and then sequentially carbonizing, densifying and purifying to obtain a carbon-carbon composite material; the mass ratio of the carbon fiber powder, carbon fiber chopped strands, phenolic resin powder, silicon carbide and liquid phenolic resin is 1:(8-10):(7-9):(0.5-1.5):(0.5-1.5); the carbonization process is specifically as follows: Treat at 800℃~900℃ for 1h~2h under nitrogen environment protection.

2. The method for treating carbon-carbon composite waste according to claim 1, characterized in that: The grinding fineness in step a) is 100-400 mesh.

3. The method for treating carbon-carbon composite waste according to claim 1, characterized in that: The carbon fiber chopped strands in step b) are obtained by crushing carbon fiber waste; the carbon fiber waste includes scraps generated in the process of weaving carbon fiber cloth and web tires generated in the process of weaving carbon fiber cloth.

4. The method for treating carbon-carbon composite waste according to claim 3, characterized in that: The length of the crushing process is 10mm~100mm.

5. The method for treating carbon-carbon composite waste according to claim 1, characterized in that: The mixing method in step b) is stirring; the stirring temperature is 10° C. to 40° C., the rotation speed is 60 r / min to 80 r / min, and the time is 20 min to 40 min.

6. The method for treating carbon-carbon composite waste according to claim 1, characterized in that: The temperature of the hot pressing molding in step b) is 150° C. to 180° C., the pressure is 5 MPa to 10 MPa, and the time is 3600 s to 7200 s.

7. The method for treating carbon-carbon composite waste according to claim 1, characterized in that: The densification in step b) adopts liquid phase impregnation phenolic resin-carbonization technology, and after impregnation with resin, it is treated at 800°C~900°C for 1h~2h under nitrogen environment protection, and repeated 2 to 4 times; the purification is treated at 2300°C~2400°C for 1h~2h under argon environment protection.