A composition for liquid waterproofing coiled material, a liquid waterproofing coiled material and a preparation method and application thereof
By using liquid waterproof coil composition in complex and narrow spaces, combined with liquid ethylene-propylene rubber and crosslinking agents, a high-strength waterproof film is formed, which solves construction difficulties and water leakage problems in the existing technology, and achieves easy construction and excellent construction waterproof effect.
Patent Information
- Application Number
- CN202410413903.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-08
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-04-08
AI Technical Summary
The existing polymer waterproof coils have construction difficulties and water leakage problems in spaces with complex and narrow construction environment, resulting in leakage, and solid coils are inconvenient for construction in narrow spaces.
Use liquid waterproof coil composition, including component A and component B, which contains liquid ethylene propylene rubber, end-hydroxyl polybutadiene, carbon noxanhydrogenated petroleum resin and carbon pentahydrogenated petroleum resin, group B It contains cross-linking accelerator and cross-linking agent, and forms a high-strength waterproof film through mixing and cross-linking, which is suitable for construction in complex and narrow spaces.
It realizes liquid waterproof coils that are easy to construct in complex and narrow spaces, has good waterproofing effect and excellent aging resistance, and improves construction efficiency and waterproof quality.
Smart Images

Figure BDA0004780171210000071 
Figure BDA0004780171210000081 
Figure BDA0004780171210000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer building waterproof materials, and in particular to a composition for liquid waterproof coiled material, a liquid waterproof coiled material, and a preparation method and application thereof. Background Art
[0002] At present, roof and underground polymer waterproof membranes are mainly constructed in the form of solid membrane paving, which is not convenient for construction in harsh and narrow spaces. Moreover, the length of each membrane is fixed and must be manually overlapped. When there are some construction defects at the overlap of the membranes, leaks will occur, leading to leakage.
[0003] Existing polymer waterproof membranes are mainly in solid state and are spread on construction sites in rolls. When the construction area is complex and narrow, construction becomes difficult, labor and time are wasted, and there may be property losses due to water seepage and leakage.
[0004] CN115806770A discloses a two-component waterproof coating and a preparation method, which is formed by a mixed reaction of component A and component B, wherein component A is: 40 to 50 parts by weight of terminal hydroxyl polybutadiene; 20 to 30 parts by weight of liquid rubber; 16 to 26 parts by weight of tackifying resin; 4 to 14 parts by weight of polyisocyanate; component B is: 59 to 69 parts by weight of terminal hydroxyl polybutadiene; 13 to 23 parts by weight of liquid rubber; 13 to 23 parts by weight of tackifying resin. This prior art utilizes the highly active hydroxyl group of terminal hydroxyl polybutadiene and uses polyisocyanate as a chain extension group to prepare an adhesive suitable for bonding polymer waterproof coiled materials. Although the overlapping points of the waterproof coiled materials after bonding have good waterproof and anti-water leakage performance, there is also the problem of construction difficulties when facing a complex and narrow construction area.
[0005] Therefore, there is an urgent need for a new type of polymer liquid waterproof membrane that is easy to construct and has excellent performance to solve this defective situation. Summary of the invention
[0006] The purpose of the present invention is to provide a liquid waterproofing coiled material which is easy to construct, has good waterproofing effect, and has super strong mechanical properties and excellent aging resistance.
[0007] In order to achieve the above object, the first aspect of the present invention provides a composition for a liquid waterproof roll material, the composition comprising component A and component B, and the weight ratio of the component A to the component B is 100:0.3-0.8;
[0008] The component A contains: 25 parts by weight of liquid ethylene-propylene rubber, 10-20 parts by weight of hydroxyl-terminated polybutadiene, 12-20 parts by weight of carbon nine hydrogenated petroleum resin, 6-12 parts by weight of carbon five hydrogenated petroleum resin, 15-30 parts by weight of filler, and 0.4-0.8 parts by weight of antioxidant;
[0009] The B component contains a crosslinking accelerator and a crosslinking agent, and the weight ratio of the crosslinking accelerator to the crosslinking agent is 1:1.6-9;
[0010] The liquid ethylene-propylene rubber has an ENB structural unit content of 8-12 wt %, an ethylene structural unit content of 30-50 wt %, and a weight average molecular weight of 30,000-50,000.
[0011] The second aspect of the present invention provides a method for preparing a liquid waterproofing membrane, which is carried out using the components in the composition described in the first aspect; the method comprises:
[0012] Mixing component A and component B in a weight ratio of 100:0.3-0.8 to obtain the liquid waterproofing membrane;
[0013] The preparation method of the A component comprises:
[0014] S1: first mixing terminal hydroxyl polybutadiene, C9 hydrogenated petroleum resin, C5 hydrogenated petroleum resin, filler and antioxidant to obtain mixture I;
[0015] S2: performing a second mixing of the mixture I and liquid ethylene-propylene rubber to obtain the component A;
[0016] The preparation method of the B component comprises:
[0017] The crosslinking accelerator and the crosslinking agent are first contacted to obtain the B component.
[0018] The third aspect of the present invention provides a liquid waterproofing membrane prepared by the method described in the second aspect.
[0019] The fourth aspect of the present invention provides application of the liquid waterproof membrane described in the third aspect in the field of building waterproofing.
[0020] The present invention sprays or pours the slurry used to form the liquid waterproofing membrane on construction defect sites or narrow spaces that are difficult to construct, and forms a layer of high-strength polymer waterproofing membrane through its own internal reaction and cross-linking, which can not only provide a waterproof effect, but also have the excellent properties of solid polymer waterproofing membrane such as aging resistance and high strength.
[0021] Liquid EPDM rubber that meets specific requirements is applied to liquid waterproof membrane, and then combined with a cross-linking agent, a cross-linking promoter, and specific terminal hydroxyl polymers, C9 hydrogenated petroleum resins, and C5 hydrogenated petroleum resins as polymer fillers to prepare a liquid waterproof membrane that is easy to construct, has good waterproofing effects, and has superb mechanical properties and excellent aging resistance. DETAILED DESCRIPTION
[0022] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0023] In the present invention, the average particle size refers to the average diameter of particles.
[0024] It should be noted that, in various aspects of the present invention, for the same components or terms in various aspects, the present invention is described only once in one aspect without repeated description, which should not be understood by those skilled in the art as a limitation of the present invention.
[0025] As mentioned above, the first aspect of the present invention provides a composition for a liquid waterproof roll material, the composition comprising component A and component B, and the weight ratio of the component A to the component B is 100:0.3-0.8;
[0026] The component A contains: 25 parts by weight of liquid ethylene-propylene rubber, 10-20 parts by weight of hydroxyl-terminated polybutadiene, 12-20 parts by weight of carbon nine hydrogenated petroleum resin, 6-12 parts by weight of carbon five hydrogenated petroleum resin, 15-30 parts by weight of filler, and 0.4-0.8 parts by weight of antioxidant;
[0027] The B component contains a crosslinking accelerator and a crosslinking agent, and the weight ratio of the crosslinking accelerator to the crosslinking agent is 1:1.6-9;
[0028] The liquid ethylene-propylene rubber has an ENB structural unit content of 8-12 wt %, an ethylene structural unit content of 30-50 wt %, and a weight average molecular weight of 30,000-50,000.
[0029] The ENB structural unit described in the present invention refers to an ethylidene norbornene structural unit.
[0030] Preferably, the component A contains: 25 parts by weight of liquid ethylene-propylene rubber, 14-18 parts by weight of hydroxyl-terminated polybutadiene, 15-20 parts by weight of carbon nine hydrogenated petroleum resin, 8-10 parts by weight of carbon five hydrogenated petroleum resin, 19-27 parts by weight of filler, and 0.6-0.8 parts by weight of antioxidant. The inventors found that the liquid waterproofing membrane prepared under the preferred conditions has better aging resistance and higher mechanical strength.
[0031] Preferably, the liquid EPDM rubber is T67 from American Lion Chemical.
[0032] Preferably, the hydroxyl value of the hydroxyl-terminated polybutadiene is 0.4-0.6 mmol / g, and the viscosity at 40°C is 8-10 Pa·s. The inventors have found in their research that by using the hydroxyl-terminated polybutadiene under the preferred conditions, combined with a specific type of liquid ethylene-propylene rubber and the other technical features of the present solution, a liquid waterproofing membrane with stronger mechanical properties and better aging resistance can be prepared.
[0033] Particularly preferably, the hydroxy-terminated polybutadiene is HTPB-I produced by Zibo Qilong Chemical Co., Ltd.
[0034] Preferably, the weight ratio of the carbon nine hydrogenated petroleum resin to the carbon five hydrogenated petroleum resin is 1:0.5-0.7. The inventors of the present invention have found in their research that by using both carbon nine hydrogenated petroleum resin and carbon five hydrogenated petroleum resin as necessary components in the composition for liquid waterproofing membrane, and controlling the usage ratio of the two under the preferred conditions, a synergistic effect can be achieved, so that the prepared liquid waterproofing membrane has better durability and mechanical strength.
[0035] Preferably, the softening points of the C9 hydrogenated petroleum resin and the C5 hydrogenated petroleum resin are independently 90-100°C.
[0036] More preferably, the carbon nine hydrogenated petroleum resin is H9-90 produced by Puyang Hengtai Petrochemical Co., Ltd.
[0037] More preferably, the C5 hydrogenated petroleum resin is H5-90 produced by Puyang Hengtai Petrochemical Co., Ltd.
[0038] Preferably, the filler includes kaolin and white carbon black.
[0039] More preferably, the filler comprises kaolin and white carbon black, and relative to 25 parts by weight of the liquid EPDM rubber, the amount of the kaolin is 10-20 parts by weight, and the amount of the white carbon black is 5-10 parts by weight.
[0040] Preferably, the average particle size of the kaolin particles is 0.5-1 μm.
[0041] Preferably, the white carbon black is a hydrophobic fumed white carbon black having a nitrogen adsorption specific surface area of 120-160 m 2 / g.
[0042] More preferably, the white carbon black is HB-615 produced by Hubei Huifu Nanomaterials Co., Ltd.
[0043] Preferably, the antioxidant is selected from at least one of German LANXESS BHT264, BASF antioxidants 1520 and 1726.
[0044] Preferably, the weight ratio of the crosslinking accelerator to the crosslinking agent in component B is 1:3-5.
[0045] Preferably, the cross-linking agent is selected from at least one of dibenzoyl peroxide, tert-butyl hydroperoxide and di-tert-butyl peroxide.
[0046] Preferably, the crosslinking accelerator is selected from at least one of aminosilanes, epoxysilanes and methacryloxysilanes.
[0047] Particularly preferably, the cross-linking accelerator is selected from at least one of Shin-Etsu KBM-903, Shin-Etsu KBM-403 and Shin-Etsu KBM-503.
[0048] As mentioned above, the second aspect of the present invention provides a method for preparing a liquid waterproofing membrane, which is carried out using the components in the composition described in the first aspect; the method comprises:
[0049] Mixing component A and component B in a weight ratio of 100:0.3-0.8 to obtain the liquid waterproofing membrane;
[0050] The preparation method of the A component comprises:
[0051] S1: first mixing terminal hydroxyl polybutadiene, C9 hydrogenated petroleum resin, C5 hydrogenated petroleum resin, filler and antioxidant to obtain mixture I;
[0052] S2: performing a second mixing of the mixture I and liquid ethylene-propylene rubber to obtain the component A;
[0053] The preparation method of the B component comprises:
[0054] The crosslinking accelerator and the crosslinking agent are first contacted to obtain the B component.
[0055] Preferably, in step S2, the temperature of the second mixing is 10-80°C, and the stirring speed is 30-50 rpm.
[0056] According to a preferred specific implementation manner, the method described in step S2 specifically comprises: introducing the mixture I into the reaction system formed with the liquid ethylene-propylene rubber at least twice to perform the second mixing.
[0057] More preferably, the mixture I is introduced into the reaction system formed with the liquid ethylene-propylene rubber in three times to carry out the second mixing.
[0058] Preferably, the weight ratio of the mixture I introduced into the reaction system for the first time, the second time and the third time is 1:0.5-1:1-1.5.
[0059] Preferably, the intervals between the first, second and third introductions of the mixture I into the reaction system are independently 20-30 min.
[0060] Preferably, in step S2, the second mixing time is 0.1-0.2 h.
[0061] The time of the second mixing described in the present invention starts from the time when the mixture I is completely introduced into the reaction system.
[0062] The present invention has no particular limitation on the conditions for performing the first mixing and the first contacting. Those skilled in the art may select the conditions according to technical means known in the art, as long as the effect of uniform mixing can be achieved. The present invention will not be elaborated herein, and those skilled in the art should not interpret it as a limitation on the present invention.
[0063] The component A and component B prepared by the method of the present invention need to be packaged separately when sold and used in a ready-to-use manner. The component A and the component B are mixed in a specific ratio to obtain a liquid waterproofing coiled material slurry, which is applied to the construction site and preferably allowed to react for ≥24 hours to obtain a finished liquid waterproofing coiled material.
[0064] Preferably, relative to 1m 3 For the base surface to be constructed, the amount of the liquid waterproof membrane slurry is 1.2-1.5kg.
[0065] As mentioned above, the third aspect of the present invention provides a liquid waterproofing membrane prepared by the method described in the second aspect.
[0066] Preferably, the liquid waterproof membrane has a tensile strength of ≥28 MPa, a puncture resistance of ≥360 N, a heat aging tensile retention rate of ≥95%, and a peeling strength between untreated and post-cast concrete of ≥1.8 N / mm.
[0067] As mentioned above, the fourth aspect of the present invention provides the application of the liquid waterproof membrane described in the third aspect in the field of building waterproofing.
[0068] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, the raw materials are all commercially available. The sources of the raw materials are shown in Table 1.
[0069] Table 1
[0070]
[0071]
[0072] In the following examples, each part by weight represents 1 kg.
[0073] Example 1
[0074] Preparation of component A:
[0075] S1: performing a first mixing (30 rpm, 0.5 h) of hydroxy-terminated polybutadiene, C9 hydrogenated petroleum resin, C5 hydrogenated petroleum resin, kaolin, white carbon black and an antioxidant to obtain a mixture I;
[0076] S2: liquid ethylene propylene rubber is placed in a stirred tank for mixing and processing, and then the mixture I is added three times, the weight ratio of the first, second and third additions is 1:0.5:1.5, the interval time is 30 minutes, and the liquid ethylene propylene rubber is mixed for the second time (40rpm, 50°C, 0.5h) to obtain component A;
[0077] Preparation of component B:
[0078] The crosslinking accelerator and the crosslinking agent are first contacted to obtain the B component.
[0079] Component A and component B are mixed in a weight ratio of 100:0.5 to obtain a liquid waterproofing membrane slurry.
[0080] The types and amounts of each component are listed in Table 2.
[0081] Example 2-3
[0082] The process is similar to that of Example 1, except that the types, amounts and operating conditions of the components are different, as shown in Table 2.
[0083] Example 4
[0084] The process is similar to that of Example 1, except that the hydroxy-terminated polybutadiene I is replaced by an equal weight portion of hydroxy-terminated polybutadiene II;
[0085] A liquid waterproofing coiled material slurry is prepared.
[0086] Example 5
[0087] The process is similar to that of Example 1, except that in step S2, the mixture I is added to the reaction system at one time, specifically:
[0088] S2: placing the liquid EPDM rubber in a stirring tank for mixing, and then adding the mixture I and the liquid EPDM rubber for a second mixing (40 rpm, 50° C., 1 h) to obtain component A;
[0089] The rest remain unchanged to prepare the liquid waterproof membrane slurry.
[0090] Example 6
[0091] The process was similar to that of Example 1, except that the stirring rate of the second mixing was adjusted from 40 rpm to 70 rpm, and the temperature and time were kept unchanged;
[0092] A liquid waterproofing coiled material slurry is prepared.
[0093] Comparative Example 1
[0094] The process is similar to that of Example 1, except that 20 parts by weight of C9 hydrogenated petroleum resin and 10 parts by weight of C5 hydrogenated petroleum resin are replaced with 30 parts by weight of C9 hydrogenated petroleum resin;
[0095] A liquid waterproofing coiled material slurry is prepared.
[0096] Comparative Example 2
[0097] The process is similar to that of Example 1, except that the liquid ethylene-propylene rubber I is replaced by an equal weight portion of liquid ethylene-propylene rubber II;
[0098] A liquid waterproofing coiled material slurry is prepared.
[0099] Table 2
[0100]
[0101] Test Case
[0102] The prepared liquid waterproofing membrane slurry was sprayed on the concrete base surface for 48 hours. 2 The base surface was sprayed with 1.2 kg of liquid waterproofing membrane slurry to obtain a finished liquid waterproofing membrane. The performance test was carried out in accordance with GB / T23457-2017. The results are shown in Table 3.
[0103] Table 3
[0104]
[0105] It can be seen from the above results that the liquid waterproof membrane of the present invention has more excellent mechanical properties and aging resistance. At the same time, the liquid waterproof membrane provided by the present invention can solve specific engineering scenarios that are not convenient for the construction of solid polymer waterproof membranes, improve the waterproof quality and application construction scenarios of the entire waterproof detail nodes of the polymer membrane, and improve the construction efficiency.
[0106] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A composition for liquid waterproofing roll, characterized in that: The composition contains component A and component B, and the weight ratio of component A to component B is 100:0.3-0.8; The component A contains: 25 parts by weight of liquid ethylene-propylene rubber, 10-20 parts by weight of hydroxyl-terminated polybutadiene, 12-20 parts by weight of carbon nine hydrogenated petroleum resin, 6-12 parts by weight of carbon five hydrogenated petroleum resin, 15-30 parts by weight of filler, and 0.4-0.8 parts by weight of antioxidant; The B component contains a crosslinking accelerator and a crosslinking agent, and the weight ratio of the crosslinking accelerator to the crosslinking agent is 1:1.6-9; The liquid ethylene-propylene rubber has an ENB structural unit content of 8-12 wt %, an ethylene structural unit content of 30-50 wt %, and a weight average molecular weight of 30,000-50,000; The hydroxyl value of the hydroxy-terminated polybutadiene is 0.4-0.6 mmol / g, and the viscosity at 40° C. is 8-10 Pa·s; The weight ratio of the carbon nine hydrogenated petroleum resin to the carbon five hydrogenated petroleum resin is 1:0.5-0.
7.
2. The composition according to claim 1, characterized in that The softening points of the C9 hydrogenated petroleum resin and the C5 hydrogenated petroleum resin are independently 90-100°C.
3. The composition according to claim 1 or 2, characterized in that The fillers include kaolin and white carbon black.
4. The composition according to claim 3, characterized in that The average particle size of the kaolin particles is 0.5-1 μm.
5. The composition according to claim 3, characterized in that The white carbon black is a hydrophobic fumed white carbon black, and the nitrogen adsorption specific surface area is 120-160m 2 / g.
6. The composition according to claim 1 or 2, characterized in that The cross-linking agent is selected from at least one of dibenzoyl peroxide, tert-butyl hydroperoxide, and di-tert-butyl peroxide; And / or, the cross-linking accelerator is selected from at least one of aminosilanes, epoxysilanes and methacryloxysilanes.
7. A method for preparing a liquid waterproofing roll, characterized in that: The method is carried out using the components in the composition according to any one of claims 1 to 6; the method comprises: Mixing component A and component B in a weight ratio of 100:0.3-0.8 to obtain the liquid waterproofing membrane; The preparation method of the A component comprises: S1: first mixing terminal hydroxyl polybutadiene, C9 hydrogenated petroleum resin, C5 hydrogenated petroleum resin, filler and antioxidant to obtain mixture I; S2: performing a second mixing of the mixture I and liquid ethylene-propylene rubber to obtain the component A; The preparation method of the B component comprises: The crosslinking accelerator and the crosslinking agent are first contacted to obtain the B component.
8. The method according to claim 7, characterized in that In step S2, the temperature of the second mixing is 10-80°C, and the stirring speed is 30-50 rpm.
9. The method according to claim 7 or 8, characterized in that: The method described in step S2 specifically includes: introducing the mixture I into the reaction system formed with the liquid ethylene-propylene rubber at least twice to perform the second mixing.
10. The method according to claim 7 or 8, characterized in that: The mixture I is introduced into the reaction system formed with the liquid ethylene-propylene rubber three times to carry out the second mixing.
11. A liquid waterproofing roll prepared by the method according to any one of claims 7 to 10.
12. Use of the liquid waterproofing membrane according to claim 11 in the field of building waterproofing.