Electrothermal response flexible tactile sensor based on carbon nanomaterials and preparation method thereof

Through an electrothermal response flexible tactile sensor based on carbon nanomaterials, the solution dispersion and impregnation technology of chitin nanocrystals and carbon nanotubes is used to solve the problem of narrow sensor sensing range and low sensitivity, achieving high sensitivity and wide sensing range and expand the scope of application.

CN118209228BActive Publication Date: 2024-11-26WUHAN TEXTILE UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410094629.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-23
Publication Date
2024-11-26
Estimated Expiration
2044-01-23

AI Technical Summary

Technical Problem

The existing flexible sensors have narrow sensing range, low sensitivity, complex preparation process and single functions, making it difficult to meet the application needs in multiple and complex environments.

Method used

Using an electrothermal response flexible tactile sensor based on carbon nanomaterials, ultrasonic dispersion is performed by preparing a solution of chitin nanocrystals and carbon nanotubes, impregnating it onto a flexible foam matrix, and forming a conductive coating through freeze-drying, combining with conductive materials to prepare A sensor with high sensitivity and wide sensing range is produced.

Benefits of technology

It achieves high sensitivity in the pressure sensing range of 0~63kPa, with a sensitivity of up to 0.374kPa-1, and has temperature change response capabilities. It is suitable for medical care and bionic human-computer interaction and other fields, with lightweight, low cost and good stability. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118209228B_ABST
    Figure CN118209228B_ABST
Patent Text Reader

Abstract

The present application provides an electrothermal responsive flexible tactile sensor based on carbon nanomaterials and a preparation method thereof, which belongs to the field of flexible sensor technology and includes the following steps: preparing a solution containing chitin nanocrystals and carbon nanotubes, and uniformly dispersing by ultrasonic dispersion to obtain a chitin nanocrystal liquid phase dispersed carbon nanotube aqueous dispersion; placing a flexible foam matrix into the chitin nanocrystal liquid phase dispersed carbon nanotube aqueous dispersion for immersion treatment, and then freeze-drying to obtain a flexible tactile sensor precursor; connecting a conductive material to the flexible tactile sensor precursor to obtain a flexible tactile sensor. The flexible tactile sensor prepared in the present application has the advantages of light weight, wide sensing range, high sensitivity, good stability, and low cost. In the pressure sensing range of 0 to 63 kPa, the sensitivity is as high as 0.374 kPa. ‑1 In the field of tactile applications, in addition to stress perception, temperature change response can also be generated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of flexible sensors, and more specifically, to an electrothermal response flexible tactile sensor based on carbon nanomaterials and a preparation method thereof. Background Art

[0002] In recent years, with the rapid development of artificial intelligence, electronic information technology and Internet of Things technology, various intelligent flexible electronic sensors have emerged and penetrated into various fields, such as medical diagnosis, smart portable devices, artificial intelligence, bionic robots, etc. Sensing technology is an indispensable and important part of intelligent development, especially high-sensitivity and high-stability sensing substrates. In order to meet the application needs of diverse and complex environments, higher requirements are put forward for the performance parameters such as the measurable range, sensitivity and stability of sensors. Traditional sensors have shortcomings such as rigidity, discomfort to wear, and difficulty in fitting tightly, resulting in inaccurate data. The transition to a new generation of flexible sensors is an inevitable trend. The development of new processes, new materials and new multifunctional flexible sensors is used as an entry point to realize the interconnection of various information and meet the needs of miniaturization, flexibility, application scenarios and functional diversification of detection equipment. Summary of the invention

[0003] The purpose of this application is to provide an electrothermal response flexible tactile sensor based on carbon nanomaterials and a preparation method thereof. The prepared flexible tactile sensor has the advantages of light weight, wide sensing range, high sensitivity, good stability, low cost, etc. In the pressure sensing range of 0 to 63 kPa, the sensitivity is as high as 0.374 kPa-1. In the field of tactile application, in addition to stress perception, it can also generate temperature change response, realize visualization of tactile contact parts, and has great application potential and development prospects in medical care and bionic human-computer interaction.

[0004] To achieve the above-mentioned object, in a first aspect of the present application, a method for preparing an electrothermal responsive flexible tactile sensor based on carbon nanomaterials is provided, comprising the following steps:

[0005] A solution containing chitosan nanocrystals and carbon nanotubes is prepared, and ultrasonic dispersion is performed to uniformly obtain a chitosan nanocrystal liquid phase dispersed carbon nanotube aqueous dispersion;

[0006] The flexible foam substrate is placed in the chitosan nanocrystal liquid phase dispersed carbon nanotube aqueous dispersion for immersion treatment, and then freeze-dried to obtain a flexible tactile sensor precursor;

[0007] A conductive material is connected to the flexible tactile sensor precursor to obtain a flexible tactile sensor.

[0008] Furthermore, in the chitosan nanocrystal liquid-phase dispersed carbon nanotube aqueous dispersion, the mass ratio of the chitosan nanocrystals to the carbon nanotubes is 0.2:1 to 9:1, and the concentration of the carbon nanotubes is 1 to 10 mg / mL.

[0009] Furthermore, the freeze-drying time after the immersion treatment is 12 to 48 hours.

[0010] Furthermore, the ultrasonic time is 30 to 120 minutes, the ultrasonic power is 300 to 500w, and after ultrasonic dispersion, centrifugal separation is performed at 3000 to 5000rpm for 10 to 30 minutes, and the chitosan nanocrystal liquid phase dispersed carbon nanotube aqueous dispersion is obtained after removing the precipitate.

[0011] Furthermore, the immersion treatment time is 5 to 30 minutes, the immersion temperature is 20 to 50° C., and after immersion, the immersion is compressed and squeezed 50 to 70% three times to squeeze out the excess chitosan nanocrystal liquid phase dispersed carbon nanotube aqueous dispersion.

[0012] Furthermore, the chitosan nanocrystals are prepared by the following method:

[0013] Chitosan powder is added into HCl solution and heated for reaction. After the reaction, the product is washed with water, dialyzed to a pH value of 7, and then freeze-dried to obtain the chitosan nanocrystals.

[0014] Furthermore, the concentration of the HCl solution used is 3-5 mol / L, and the concentration of the chitosan powder in the HCl solution is 20-50 mg / ml.

[0015] Furthermore, after the heating reaction is completed, deionized water is added and centrifuged at high speed for multiple times until the pH value is 3, and then dialyzed for 4 to 7 days until the pH value of the dialysate is 7, followed by freeze-drying for 12 to 48 hours.

[0016] Furthermore, the temperature of the heating reaction is 95-105° C., and the reaction time is 6-8 hours.

[0017] Furthermore, the step of connecting the conductive material to the flexible tactile sensor precursor is: pasting conductive wires on the upper and lower surfaces of the flexible tactile sensor precursor with insulating tape.

[0018] Furthermore, the flexible foam matrix is ​​any one of melamine foam, polyurethane foam, melamine foam, polyethylene foam and polypropylene foam, and its porosity is 95-98%.

[0019] In a second aspect of the present application, there is provided an electrothermal responsive flexible tactile sensor based on carbon nanomaterials, which is obtained by any of the preparation methods described above.

[0020] Compared with the prior art, this application has the following technical effects:

[0021] The present invention discloses a method for preparing an electrothermal responsive flexible tactile sensor based on carbon nanomaterials. The method uses chitin nanocrystals (CNW) to disperse carbon nanotubes (CNTs) in a liquid phase to form π-π conjugated non-covalent bonds to modify the CNT surface and improve its dispersibility, thereby obtaining a stable chitin nanocrystal liquid phase dispersed carbon nanotube aqueous dispersion (CCNT dispersion). The CCNTs are then adsorbed on the skeleton surface of a flexible foam substrate by an immersion-freeze drying method to form a conductive coating of the CCNTs. Finally, a conductive material is connected to the flexible foam substrate to prepare an electrothermal responsive flexible tactile sensor based on carbon nanomaterials.

[0022] The flexible tactile sensor prepared in this application has the advantages of light weight, wide sensing range, high sensitivity, good stability, and low cost. In the pressure sensing range of 0 to 63 kPa, the sensitivity is as high as 0.374 kPa. -1 In the field of tactile applications, in addition to stress perception, it can also generate temperature change responses, realize visualization of tactile contact points, and has great application potential and development prospects in medical care and bionic human-computer interaction. It solves the current problems of flexible sensors such as narrow sensing range, low sensitivity, complex preparation process, and single function, and expands the scope of application.

[0023] The chitosan used in this application is a degradable biomass material with good antibacterial activity and biocompatibility, and is green and environmentally friendly; the surface of CNW contains a large number of conjugated groups and hydrophilic amide groups and hydroxyl groups. Through simple ultrasonic dispersion, a layer of CNW can be wrapped around the CNT, and the CNT can be evenly and stably dispersed in the aqueous solution; and the impregnation method used is a low-cost and high-efficiency loading method; the freeze-drying method can ensure that the CCNT coating is evenly and stably coated on the three-dimensional skeleton surface of the flexible foam matrix. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0025] Figure 1 A flow chart of a method for preparing an electrothermal responsive flexible tactile sensor based on carbon nanomaterials provided in an embodiment of the present application;

[0026] Figure 2 The conductivity bar graph of CCNT dispersions with different feed ratios in implementations 1-6 of this application;

[0027] Figure 3 This is a sensitivity curve diagram of the electrothermal response flexible tactile sensor based on carbon nanomaterials prepared in Example 4 of the present application;

[0028] Figure 4 The scanning electron microscope images of the melamine foam before (upper figure), after (lower figure) loading CCNT and its local magnification in Example 4 of the present application;

[0029] Figure 5 This is a stress-strain curve diagram of the electrothermal response flexible tactile sensor based on carbon nanomaterials prepared in Example 4 of the present application;

[0030] Figure 6 This is a graph showing the stability of the resistance change rate of the electrothermal response flexible tactile sensor based on carbon nanomaterials prepared in Example 4 of the present application at different pressure rates under a stress of 30 kPa;

[0031] Figure 7 This is a cyclic stability curve of the electrothermal response flexible tactile sensor based on carbon nanomaterials prepared in Example 4 of the present application under a pressure of 30 kPa;

[0032] Figure 8 The graph of the relationship between temperature and voltage under different compressive stresses is a graph of the electrothermal performance of the electrothermal responsive flexible tactile sensor based on carbon nanomaterials prepared in Example 4 of the present application;

[0033] Fig. 9 A schematic diagram of the electrothermal temperature of the electrothermal responsive flexible tactile sensor based on carbon nanomaterials prepared in Example 4 of the present application under different pressures and different voltages;

[0034] Fig.10 This is a temperature change curve of the electrothermal response flexible tactile sensor based on carbon nanomaterials prepared in Example 4 of the present application after loading a 5V voltage under a stress of 63kPa. DETAILED DESCRIPTION

[0035] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0036] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0037] The weight of the relevant components mentioned in the specification of the examples of this application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the specification of the examples of this application, it is within the scope disclosed in the specification of the examples of this application. Specifically, the mass described in the specification of the examples of this application can be a mass unit known in the biochemical field such as μg, mg, g, kg, etc.

[0038] The present application provides an electrothermal response flexible tactile sensor based on carbon nanomaterials and a preparation method thereof. The preparation process is as follows: Figure 1 As shown, it mainly includes the following four steps:

[0039] (1) Selection and pretreatment of lightweight flexible foam substrate;

[0040] (2) Selection and preparation of dispersants;

[0041] (3) Preparation of chitin nanocrystal (CNW) liquid-dispersed carbon nanotube (CNT) aqueous dispersion (CCNT);

[0042] (4) Construction of flexible tactile sensors.

[0043] In the above step (1), the lightweight flexible foam substrate is a polymer foam with a three-dimensional skeleton network structure having an ultra-high porosity of 95-98%, and can be any one of melamine foam, polyurethane foam, melamine foam, polyethylene foam, and polypropylene foam.

[0044] The pretreatment process of the lightweight flexible foam substrate is: first, the lightweight flexible foam substrate is cleaned in an ultrasonic cleaner with deionized water for 10-30 minutes to remove impurities, and then refluxed in a Soxhlet extractor with acetone for 4-8 times to remove organic matter adhering to the surface.

[0045] In the above step (2), the selected dispersant is the biomass material chitosan, and the desired nano-scale material CNW is prepared by acid hydrolysis. The acid hydrolysis method is mainly used to prepare CNW with a low aspect ratio. Stirring at high temperature for a certain period of time in an acid solution can cause the amorphous region in the chitosan to expand and acidify, while the high crystalline region remains intact. The large pieces of chitosan are decomposed into the desired nano-scale material, and then CNW is obtained by dialysis and freeze drying. The temperature of the acid hydrolysis heating reaction is 95-105°C, and the reaction time is 6-8h. HCl is generally used for acid hydrolysis.

[0046] In the above step (3), the preparation of CCNT aqueous dispersion is carried out by ultrasonic liquid phase dispersion method, the CNW and CNT prepared above are dispersed in aqueous solution, ultrasonic dispersion is carried out by ultrasonic probe, and the undispersed CNT is removed by centrifugation after ultrasonication to obtain CCNT aqueous dispersion; wherein, the feed ratio of CNW and CNT is 0.2:1-9:1, stirring for 5-20 minutes to fully mix, the ultrasonic time is 30-120 minutes, the ultrasonic power is 300-500w, after ultrasonic dispersion, centrifugation is carried out at 3000-5000rpm for 10-30 minutes, and the precipitate is removed. The concentration of CNT in the prepared aqueous dispersion is 1-10mg / mL. Preferably, the feed ratio of CNW and CNT for the best dispersion effect is 1:1.

[0047] In the above step (4), the CCNT in the above (3) is coated on the surface of the polymer foam by an impregnation-freeze drying method to form a conductive network. The impregnation time is 5 to 30 minutes, the impregnation temperature is 20 to 50°C, and after impregnation, it is compressed and squeezed 50 to 70% three times, and the excess CCNT aqueous dispersion is squeezed out. Then, it is refrigerated and frozen for 24 to 36 hours, and the freeze drying time is 12 to 48 hours. Finally, conductive wires are attached to the upper and lower surfaces with insulating tape to complete the preparation of an electrothermal response flexible tactile sensor based on carbon nanomaterials.

[0048] The following uses a plurality of specific embodiments to illustrate an electrothermal response flexible tactile sensor based on carbon nanomaterials and a preparation method thereof according to an embodiment of the present application.

[0049] Example 1

[0050] Embodiment 1 of the present application provides an electrothermal response flexible tactile sensor based on carbon nanomaterials and a preparation method thereof, comprising the following steps:

[0051] S1: The melamine foam is first cleaned with deionized water in an ultrasonic cleaner for 30 minutes to remove surface impurities; then, refluxed with acetone in a Soxhlet extractor for 6 times, and dried to obtain clean melamine foam;

[0052] S2: Preparation of dispersant CNW: Prepare 3 mol / L HCl solution, add 20 g of commercially available chitosan powder, heat to a slightly boiling state at 100°C, stir and react for 8 hours, add deionized water after the reaction and remove the solution by high-speed centrifugation at 8000 rpm for 3 times to a pH value of 3, then add the solid precipitate to deionized water and stir evenly, put the solution into a dialysis bag of 8000-14000D, and dialyze in deionized water for 4-7 days, changing the deionized water every day during the period until the pH value is 7.

[0053] S3: The dialyzed solution in S2 is refrigerated and frozen for 24 hours, and then freeze-dried. The freeze-drying treatment time is 24 hours. After freeze-drying, the desired nanoscale material CNW is obtained.

[0054] S4: Disperse the CNW prepared in S3 in deionized water. After stirring and dispersing evenly, weigh a certain amount of CNT and mix it into the solution. The concentration of CNT in the solution is fixed at 4 mg / mL, and the mass ratio of CNW to CNT is 0.5:4.

[0055] S5: The mixed solution of S4 is subjected to ultrasonic treatment. The instrument used is a probe ultrasonic cell crusher. The ultrasonic power is set to 400W. After ultrasonic treatment for 120 minutes in an ice bath, it is taken out. Due to the strong van der Waals force between CNTs, they are aggregated into clusters. The cavitation effect generated by the probe ultrasound can effectively disperse them. At the same time, CNWs in the solution are adsorbed on the surface of CNTs through π-π conjugation.

[0056] S6: centrifuging the solution obtained after the ultrasound in S5 at 4500 rpm for 10 min to remove the undispersed carbon nanotubes, taking the supernatant to obtain a CCNT aqueous dispersion;

[0057] S7: Cut the melamine foam cleaned in S1 into 2×2 cm squares, immerse them in the CNT aqueous dispersion in S6 for 30 min at a temperature of 30°C. During immersion, no external force is applied. The melamine foam is simply placed on the surface of the CCNT aqueous dispersion. The solution fully soaks the foam from bottom to top to prevent uneven loading caused by the "hollowing" phenomenon.

[0058] S8: Take out the foam after the immersion in S7, compress and squeeze the foam by 50-70% three times, squeeze out the excess CCNT aqueous dispersion, and then put the treated foam into a refrigerator for 24 hours.

[0059] S9: Place the frozen sample in the above S8 into a freeze dryer for freeze drying. The freeze drying time is 24 hours.

[0060] S10: After the sample of S9 is freeze-dried, conductive wires are attached to the upper and lower surfaces thereof with insulating tape, thereby preparing a flexible tactile sensor with electrothermal response based on carbon nanomaterials.

[0061] Example 2

[0062] Embodiment 2 of the present application provides an electrothermal response flexible tactile sensor based on carbon nanomaterials and a preparation method thereof, comprising the following steps:

[0063] S1: The melamine foam is first cleaned with deionized water in an ultrasonic cleaner for 30 minutes to remove surface impurities; then, refluxed with acetone in a Soxhlet extractor for 6 times, and dried to obtain clean melamine foam;

[0064] S2: Preparation of dispersant CNW: Prepare 3 mol / L HCl solution, add 20 g of commercially available chitosan powder, heat to a slightly boiling state at 100°C, stir and react for 8 hours, add deionized water after the reaction and remove the solution by high-speed centrifugation at 8000 rpm for 3 times to a pH value of 3, then add the solid precipitate to deionized water and stir evenly, put the solution into a dialysis bag of 8000-14000D, and dialyze in deionized water for 4-7 days, changing the deionized water every day during the period until the pH value is 7.

[0065] S3: The dialyzed solution in S2 is refrigerated and frozen for 36 hours, and then freeze-dried. The freeze-drying treatment time is 12 hours. After freeze-drying, the desired nanoscale material CNW is obtained.

[0066] S4: Disperse the CNW prepared in S3 in deionized water. After stirring and dispersing evenly, weigh a certain amount of CNT and mix it into the solution. The concentration of CNT in the solution is fixed at 4 mg / mL, and the mass ratio of CNW to CNT is 1:4.

[0067] S5: The mixed solution of S4 is subjected to ultrasonic treatment. The instrument used is a probe ultrasonic cell crusher. The ultrasonic power is set to 400W. After ultrasonic treatment for 120 minutes in an ice bath, it is taken out. Due to the strong van der Waals force between CNTs, they are aggregated into clusters. The cavitation effect generated by the probe ultrasound can effectively disperse them. At the same time, CNWs in the solution are adsorbed on the surface of CNTs through π-π conjugation.

[0068] S6: centrifuging the solution obtained after the ultrasound in S5 at 4500 rpm for 10 min to remove the undispersed carbon nanotubes, taking the supernatant to obtain a CCNT aqueous dispersion;

[0069] S7: Cut the melamine foam cleaned in S1 into 2×2 cm squares, immerse them in the CNT aqueous dispersion in S6 for 10 min at a temperature of 40°C. During immersion, no external force is applied. Simply place the melamine foam gently on the surface of the CCNT aqueous dispersion, and allow the solution to fully soak the foam from bottom to top to prevent uneven loading caused by the "hollowing" phenomenon.

[0070] S8: Take out the foam after the immersion in S7, compress and squeeze the foam by 50-70% three times, squeeze out the excess CCNT aqueous dispersion, and then put the treated foam into a refrigerator for 36 hours.

[0071] S9: Place the frozen sample in the above S8 into a freeze dryer for freeze drying. The freeze drying time is 12 hours.

[0072] S10: After the sample of S9 is freeze-dried, conductive wires are attached to the upper and lower surfaces thereof with insulating tape, thereby preparing a flexible tactile sensor with electrothermal response based on carbon nanomaterials.

[0073] Example 3

[0074] Embodiment 3 of the present application provides an electrothermal response flexible tactile sensor based on carbon nanomaterials and a preparation method thereof, comprising the following steps:

[0075] S1: The melamine foam is first cleaned with deionized water in an ultrasonic cleaner for 30 minutes to remove surface impurities; then, refluxed with acetone in a Soxhlet extractor for 6 times, and dried to obtain clean melamine foam;

[0076] S2: Preparation of dispersant CNW: Prepare 3 mol / L HCl solution, add 20 g of commercially available chitosan powder, heat to a slightly boiling state at 100°C, stir and react for 8 hours, add deionized water after the reaction and remove the solution by high-speed centrifugation at 8000 rpm for 3 times to a pH value of 3, then add the solid precipitate to deionized water and stir evenly, put the solution into a dialysis bag of 8000-14000D, and dialyze in deionized water for 4-7 days, changing the deionized water every day during the period until the pH value is 7.

[0077] S3: The dialyzed solution in S2 is refrigerated and frozen for 24 hours, and then freeze-dried. The freeze-drying treatment time is 48 hours. After freeze-drying, the desired nano-scale material CNW is obtained.

[0078] S4: Disperse the CNW prepared in S3 in deionized water. After stirring and dispersing evenly, weigh a certain amount of CNT and mix it into the solution. The concentration of CNT in the solution is fixed at 4 mg / mL, and the mass ratio of CNW to CNT is 2:4.

[0079] S5: The mixed solution of S4 is subjected to ultrasonic treatment. The instrument used is a probe ultrasonic cell crusher. The ultrasonic power is set to 400W. After ultrasonic treatment for 120 minutes in an ice bath, it is taken out. Due to the strong van der Waals force between CNTs, they are aggregated into clusters. The cavitation effect generated by the probe ultrasound can effectively disperse them. At the same time, CNWs in the solution are adsorbed on the surface of CNTs through π-π conjugation.

[0080] S6: centrifuging the solution obtained after the ultrasound in S5 at 4500 rpm for 10 min to remove the undispersed carbon nanotubes, taking the supernatant to obtain a CCNT aqueous dispersion;

[0081] S7: Cut the melamine foam cleaned in S1 into 2×2 cm squares, immerse them in the CNT aqueous dispersion in S6 for 5 min at a temperature of 50°C. During immersion, no external force is applied. The melamine foam is simply placed on the surface of the CCNT aqueous dispersion. The solution fully soaks the foam from bottom to top to prevent uneven loading caused by the "hollowing" phenomenon.

[0082] S8: Take out the foam after the immersion in S7, compress and squeeze the foam by 50-70% three times, squeeze out the excess CCNT aqueous dispersion, and then put the treated foam into a refrigerator for 36 hours.

[0083] S9: Place the frozen sample in the above S8 into a freeze dryer for freeze drying. The freeze drying time is 48 hours.

[0084] S10: After the sample of S9 is freeze-dried, conductive wires are attached to the upper and lower surfaces thereof with insulating tape, thereby preparing a flexible tactile sensor with electrothermal response based on carbon nanomaterials.

[0085] Example 4

[0086] Embodiment 4 of the present application provides an electrothermal response flexible tactile sensor based on carbon nanomaterials and a preparation method thereof, comprising the following steps:

[0087] S1: The melamine foam is first cleaned with deionized water in an ultrasonic cleaner for 30 minutes to remove surface impurities; then, refluxed with acetone in a Soxhlet extractor for 6 times, and dried to obtain clean melamine foam;

[0088] S2: Preparation of dispersant CNW: Prepare 3 mol / L HCl solution, add 20 g of commercially available chitosan powder, heat to a slightly boiling state at 100°C, stir and react for 8 hours, add deionized water after the reaction and remove the solution by high-speed centrifugation at 8000 rpm for 3 times to a pH value of 3, then add the solid precipitate to deionized water and stir evenly, put the solution into a dialysis bag of 8000-14000D, and dialyze in deionized water for 4-7 days, changing the deionized water every day during the period until the pH value is 7.

[0089] S3: The dialyzed solution in S2 is refrigerated and frozen for 24 hours, and then freeze-dried. The freeze-drying treatment time is 24 hours. After freeze-drying, the desired nanoscale material CNW is obtained.

[0090] S4: Disperse the CNW prepared in S3 in deionized water. After stirring and dispersing evenly, weigh a certain amount of CNT and mix it into the solution. The concentration of CNT in the solution is fixed at 4 mg / mL, and the mass ratio of CNW to CNT is 4:4.

[0091] S5: The mixed solution of S4 is subjected to ultrasonic treatment. The instrument used is a probe ultrasonic cell crusher. The ultrasonic power is set to 400W. After ultrasonic treatment for 120 minutes in an ice bath, it is taken out. Due to the strong van der Waals force between CNTs, they are aggregated into clusters. The cavitation effect generated by the probe ultrasound can effectively disperse them. At the same time, CNWs in the solution are adsorbed on the surface of CNTs through π-π conjugation.

[0092] S6: centrifuging the solution obtained after the ultrasound in S5 at 4500 rpm for 10 min to remove the undispersed carbon nanotubes, taking the supernatant to obtain a CCNT aqueous dispersion;

[0093] S7: Cut the melamine foam cleaned in S1 into 2×2 cm squares, immerse them in the CNT aqueous dispersion in S6 for 20 min at a temperature of 30°C. During immersion, no external force is applied. The melamine foam is simply placed on the surface of the CCNT aqueous dispersion. The solution fully soaks the foam from bottom to top to prevent uneven loading caused by the "hollowing" phenomenon.

[0094] S8: Take out the foam after the immersion in S7, compress and squeeze the foam by 50-70% three times, squeeze out the excess CCNT aqueous dispersion, and then put the treated foam into a refrigerator for 36 hours.

[0095] S9: Place the frozen sample in the above S8 into a freeze dryer for freeze drying. The freeze drying time is 12 hours.

[0096] S10: After the sample of S9 is freeze-dried, conductive wires are attached to the upper and lower surfaces thereof with insulating tape, thereby preparing a flexible tactile sensor with electrothermal response based on carbon nanomaterials.

[0097] Example 5

[0098] Embodiment 5 of the present application provides an electrothermal response flexible tactile sensor based on carbon nanomaterials and a preparation method thereof, comprising the following steps:

[0099] S1: The melamine foam is first cleaned with deionized water in an ultrasonic cleaner for 30 minutes to remove surface impurities; then, refluxed with acetone in a Soxhlet extractor for 6 times, and dried to obtain clean melamine foam;

[0100] S2: Preparation of dispersant CNW: Prepare 3 mol / L HCl solution, add 20 g of commercially available chitosan powder, heat to a slightly boiling state at 100°C, stir and react for 8 hours, add deionized water after the reaction and remove the solution by high-speed centrifugation at 8000 rpm for 3 times to a pH value of 3, then add the solid precipitate to deionized water and stir evenly, put the solution into a dialysis bag of 8000-14000D, and dialyze in deionized water for 4-7 days, changing the deionized water every day during the period until the pH value is 7.

[0101] S3: The dialyzed solution in S2 is refrigerated and frozen for 36 hours, and then freeze-dried. The freeze-drying treatment time is 48 hours. After freeze-drying, the desired nano-scale material CNW is obtained.

[0102] S4: Disperse the CNW prepared in S3 in deionized water. After stirring and dispersing evenly, weigh a certain amount of CNT and mix it into the solution. The concentration of CNT in the solution is fixed at 4 mg / mL, and the mass ratio of CNW to CNT is 6:4.

[0103] S5: The mixed solution of S4 is subjected to ultrasonic treatment. The instrument used is a probe ultrasonic cell crusher. The ultrasonic power is set to 400W. After ultrasonic treatment for 120 minutes in an ice bath, it is taken out. Due to the strong van der Waals force between CNTs, they are aggregated into clusters. The cavitation effect generated by the probe ultrasound can effectively disperse them. At the same time, CNWs in the solution are adsorbed on the surface of CNTs through π-π conjugation.

[0104] S6: centrifuging the solution obtained after the ultrasound in S5 at 4500 rpm for 10 min to remove the undispersed carbon nanotubes, taking the supernatant to obtain a CCNT aqueous dispersion;

[0105] S7: Cut the melamine foam cleaned in S1 into 2×2 cm squares, immerse them in the CNT aqueous dispersion in S6 for 10 min at a temperature of 40°C. During immersion, no external force is applied. Simply place the melamine foam gently on the surface of the CCNT aqueous dispersion, and allow the solution to fully soak the foam from bottom to top to prevent uneven loading caused by the "hollowing" phenomenon.

[0106] S8: Take out the foam after the immersion in S7, compress and squeeze the foam by 50-70% three times, squeeze out the excess CCNT aqueous dispersion, and then put the treated foam into a refrigerator for 24 hours.

[0107] S9: Place the frozen sample in the above S8 into a freeze dryer for freeze drying. The freeze drying time is 24 hours.

[0108] S10: After the sample of S9 is freeze-dried, conductive wires are attached to the upper and lower surfaces thereof with insulating tape, thereby preparing a flexible tactile sensor with electrothermal response based on carbon nanomaterials.

[0109] Example 6

[0110] Embodiment 6 of the present application provides an electrothermal response flexible tactile sensor based on carbon nanomaterials and a preparation method thereof, comprising the following steps:

[0111] S1: The melamine foam is first cleaned with deionized water in an ultrasonic cleaner for 30 minutes to remove surface impurities; then, refluxed with acetone in a Soxhlet extractor for 6 times, and dried to obtain clean melamine foam;

[0112] S2: Preparation of dispersant CNW: Prepare 3 mol / L HCl solution, add 20 g of commercially available chitosan powder, heat to a slightly boiling state at 100°C, stir and react for 8 hours, add deionized water after the reaction and remove the solution by high-speed centrifugation at 8000 rpm for 3 times to a pH value of 3, then add the solid precipitate to deionized water and stir evenly, put the solution into a dialysis bag of 8000-14000D, and dialyze in deionized water for 4-7 days, changing the deionized water every day during the period until the pH value is 7.

[0113] S3: The dialyzed solution in S2 is refrigerated and frozen for 24 hours, and then freeze-dried. The freeze-drying treatment time is 24 hours. After freeze-drying, the desired nanoscale material CNW is obtained.

[0114] S4: Disperse the CNW prepared in S3 in deionized water. After stirring and dispersing evenly, weigh a certain amount of CNT and mix it into the solution. The concentration of CNT in the solution is fixed at 4 mg / mL, and the mass ratio of CNW to CNT is 8:4.

[0115] S5: The mixed solution of S4 is subjected to ultrasonic treatment. The instrument used is a probe ultrasonic cell crusher. The ultrasonic power is set to 400W. After ultrasonic treatment for 120 minutes in an ice bath, it is taken out. Due to the strong van der Waals force between CNTs, they are aggregated into clusters. The cavitation effect generated by the probe ultrasound can effectively disperse them. At the same time, CNWs in the solution are adsorbed on the surface of CNTs through π-π conjugation.

[0116] S6: centrifuging the solution obtained after the ultrasound in S5 at 4500 rpm for 10 min to remove the undispersed carbon nanotubes, taking the supernatant to obtain a CCNT aqueous dispersion;

[0117] S7: Cut the melamine foam cleaned in S1 into 2×2 cm squares, immerse them in the CNT aqueous dispersion in S6 for 30 min at a temperature of 30°C. During immersion, no external force is applied. The melamine foam is simply placed on the surface of the CCNT aqueous dispersion. The solution fully soaks the foam from bottom to top to prevent uneven loading caused by the "hollowing" phenomenon.

[0118] S8: Take out the foam after the immersion in S7, compress and squeeze the foam by 50-70% three times, squeeze out the excess CCNT aqueous dispersion, and then put the treated foam into a refrigerator for 24 hours.

[0119] S9: Place the frozen sample in the above S8 into a freeze dryer for freeze drying. The freeze drying time is 48 hours.

[0120] S10: After the sample of S9 is freeze-dried, conductive wires are attached to the upper and lower surfaces thereof with insulating tape, thereby preparing a flexible tactile sensor with electrothermal response based on carbon nanomaterials.

[0121] Figure 2 The conductivity bar graph of CCNT dispersions with different feed ratios in implementation 1-6 of the present application shows that the conductivity of the CCNT dry film first increases and then decreases. This is because as the CNW content in the solution increases, the dispersion of CNTs becomes better, the formed dry film becomes denser and the conductivity becomes better, but CNWs are not conductive. As CNWs continue to increase, the conductivity of the CCNT dry film also decreases. Therefore, when the conductivity of the CCNT dry film is the highest, the feed ratio of CNW to CNT is the optimal feed ratio, that is, 4:4.

[0122] Figure 3 This is a sensitivity curve of the electrothermal responsive flexible tactile sensor based on carbon nanomaterials prepared in Example 4 of the present application. When pressure is applied, the internal three-dimensional skeletons are constantly in contact, the number of conductive paths increases, and the resistance is significantly reduced; as the compressive stress further increases to above 15kPa, the pores inside the foam are greatly reduced or even disappear, the number of conductive paths gradually tends to be constant, the resistance slowly decreases due to the shortening of the conductive path distance, and the resistance change rate slowly decreases. At this time, the sensitivity of the sensor is 0.374kPa -1 .

[0123] Figure 4 The scanning electron microscope images of the melamine foam before and after CCNT loading and its local magnification in Example 4 of the present application show that the melamine foam has a three-dimensional skeleton structure with a smooth surface free of impurities; and after impregnation and freeze-drying treatment, CCNT is evenly coated on the surface of the melamine foam skeleton.

[0124] Figure 5This is a stress-strain curve of the electrothermal responsive flexible tactile sensor based on carbon nanomaterials prepared in Example 4 of the present application. The ultra-high porosity of the foam makes the prepared tactile sensor have a wide strain range, and the stress reaches 63 kPa when compressed to 70%.

[0125] Figure 6 This is a resistance change rate stability curve of the carbon nanomaterial-based electrothermal response flexible tactile sensor prepared in Example 4 of the present application at different pressure rates under 30 kPa stress. The resistance change rate of the sensor is the same when the same stress is applied slowly and quickly.

[0126] Figure 7 This is a cyclic stability curve of the electrothermal responsive flexible tactile sensor based on carbon nanomaterials prepared in Example 4 of the present application under a pressure of 30 kPa. Stability is an important parameter of the sensor. The cyclic pressure test shows that the prepared flexible tactile sensor has good cyclic stability.

[0127] Figure 8 The temperature-voltage relationship curve of the electrothermal performance of the electrothermal responsive flexible tactile sensor based on carbon nanomaterials prepared in Example 4 of the present application under different compressive stresses shows that when the voltage is not higher than the human safety voltage of 24V, the temperature increases with the increase of the applied voltage. At the same time, when the same voltage is applied at both ends, the temperature increases with the increase of the compressive stress. When a pressure of 63kPa is applied and a voltage of 7V is loaded, the temperature of the sensor rises to 61.4°C.

[0128] Fig. 9 This is a schematic diagram of the electrothermal temperature of the electrothermal responsive flexible tactile sensor based on carbon nanomaterials prepared in Example 4 of the present application under different pressures and different voltages. As the applied pressure increases, the resistance of the sensor continues to decrease and the temperature gradually increases; similarly, as the loaded voltage increases, the temperature also gradually increases.

[0129] Fig.10 This is a temperature change curve of the electrothermal responsive flexible tactile sensor based on carbon nanomaterials prepared in Example 4 of the present application after loading a 5V voltage under a stress of 63kPa. Under the low-energy 5V voltage and 63kPa pressure, the temperature of the sensor is stabilized at 39.7°C.

[0130] The preparation method of a carbon nanomaterial-based electrothermal response flexible tactile sensor in an embodiment of the present application adopts chitin nanocrystals (CNW) liquid phase dispersed carbon nanotubes (CNTs) to form π-π conjugated non-covalent bonds to modify the CNT surface and improve its dispersibility, thereby obtaining a stable chitin nanocrystal liquid phase dispersed carbon nanotube aqueous dispersion (CCNT dispersion), and then adsorbing CCNT on the skeleton surface of a flexible foam substrate by an immersion-freeze drying method to form a conductive coating of CCNT, and finally connecting a conductive material (conductive tape) to the flexible foam substrate to prepare a carbon nanomaterial-based electrothermal response flexible tactile sensor.

[0131] The flexible tactile sensor based on carbon nanomaterials prepared in the embodiment of the present application has the advantages of light weight, wide sensing range, high sensitivity, good stability, low cost, etc. In the pressure sensing range of 0 to 63 kPa, the sensitivity is as high as 0.374 kPa. -1 In the field of tactile applications, in addition to stress perception, it can also generate temperature change responses and realize visualization of tactile contact points. It has great application potential and development prospects in medical care and bionic human-computer interaction.

[0132] The above embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.

Claims

1. A method for preparing an electrothermal responsive flexible tactile sensor based on carbon nanomaterials, characterized in that: The following steps are involved: A solution containing chitosan nanocrystals and carbon nanotubes is prepared, and ultrasonic dispersion is performed to obtain a chitosan nanocrystal liquid-phase dispersed carbon nanotube aqueous dispersion; in the chitosan nanocrystal liquid-phase dispersed carbon nanotube aqueous dispersion, the mass ratio of the chitosan nanocrystals to the carbon nanotubes is 0.2:1-9:1, and the concentration of the carbon nanotubes is 1-10 mg / mL; the ultrasonic time is 30-120 min, the ultrasonic power is 300-500 w, and after ultrasonic dispersion, the solution is centrifuged at 3000-5000 rpm for 10-30 min, and the precipitate is removed to obtain the chitosan nanocrystal liquid-phase dispersed carbon nanotube aqueous dispersion; The melamine foam substrate is placed in the chitosan nanocrystal liquid phase dispersed carbon nanotube aqueous dispersion for immersion treatment, and then freeze-dried to obtain a flexible tactile sensor precursor; the immersion treatment time is 5 to 30 minutes, the immersion temperature is 20 to 50 ° C, and after immersion, it is compressed and squeezed 50 to 70% three times to squeeze out the excess chitosan nanocrystal liquid phase dispersed carbon nanotube aqueous dispersion; The chitosan nanocrystals are prepared by the following method: Adding chitosan powder to HCl solution, heating reaction, washing the product with water, dialyzing to a pH value of 7, and then freeze-drying to obtain the chitosan nanocrystals; the heating reaction temperature is 95-105°C, and the reaction time is 6-8 hours; A conductive material is connected to the flexible tactile sensor precursor to obtain a flexible tactile sensor.

2. The method for preparing the electrothermal responsive flexible tactile sensor based on carbon nanomaterials according to claim 1, characterized in that: The concentration of the HCl solution used is 3-5 mol / L, and the concentration of the chitosan powder in the HCl solution is 20-50 mg / ml.

3. The method for preparing the electrothermal responsive flexible tactile sensor based on carbon nanomaterials according to claim 1, characterized in that: The step of connecting the conductive material to the flexible tactile sensor precursor is as follows: conductive wires are attached to the upper and lower surfaces of the flexible tactile sensor precursor using insulating tape.

4. An electrothermal responsive flexible tactile sensor based on carbon nanomaterials, characterized in that: The preparation method according to any one of claims 1 to 3 is used to obtain the