A preparation method of high-strength interface-bonded beryllium aluminum composite material
By using liquid silicon-based precursors in beryllium aluminum composite materials to form silicon-coated beryllium particles, the problems of low interface strength and insufficient density are solved, the mechanical properties of the material are significantly improved, and high strength and high plasticity are achieved. Preparation of beryllium aluminum composite material.
Patent Information
- Application Number
- CN202410327619.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-03-21
AI Technical Summary
The existing beryllium aluminum composite materials have low interface strength and insufficient density, resulting in failure of the material at the interface and degradation of overall performance.
Interface modification layer is formed by surface modification of beryllium powder, and heat treatment is used in a vacuum heating furnace using a liquid silicon-based precursor to decompose it in situ into silicon coated beryllium particles, and mechanical ball milling and sintering are combined with aluminum powder to form high strength Interface combined with beryllium aluminum composite material.
It significantly improves the interface bonding strength of beryllium aluminum, ensures the cleanliness and plasticity of the matrix, solves the problem of material interface cracking, and improves the mechanical properties of the material, such as interface bonding strength, bending strength, yield strength and tensile strength.
Smart Images

Figure CN118222866B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a beryllium aluminum composite material. Background Art
[0002] Beryllium is an ultra-light metal element with an atomic number of 4 and a single-substance density of only 1.85 g / cm 3 , and the elastic modulus is about 310GPa, which has the advantages of light weight and high strength. Among them, the composite of beryllium and aluminum alloy takes into account both strength and plasticity, and is considered to be an important direction for the development of beryllium materials. At present, beryllium aluminum composite materials have been used in important structures and optical devices in aerospace due to their ultra-high specific strength and specific stiffness. Among them, the beryllium aluminum interface is the key to determining the performance of the material.
[0003] Since beryllium and aluminum almost do not form a solid solution at room temperature and have a clear interface, under conventional material preparation methods, beryllium aluminum forms a simple interface without specific orientation and physical bonding by van der Waals forces. The simple beryllium aluminum interface has low bonding strength and cannot meet the stress requirements when the material is deformed, which causes the composite material to break and fail at the interface, reducing the overall performance of the material. Traditional interface regulation methods use matrix alloying to improve interface bonding through alloying elements (such as Si, Cu, Ni, etc.), but the matrix alloying method often requires the spontaneous diffusion of alloying elements in the material to the interface, and the interface regulation efficiency is low. At the same time, a large amount of alloying elements need to be added, which easily reduces the plasticity of the aluminum matrix. And because the peripheral electron configuration of beryllium metal is 2s 2 , the metallic property is low, the reaction activity is poor, and it is not easy to form a close bond with other phases. When beryllium and aluminum are directly combined, the material is difficult to densify. Therefore, a preparation method of a high-strength interface-bonded beryllium-aluminum composite material is urgently needed. Summary of the invention
[0004] In order to solve the problems of low interface strength and low density of existing beryllium aluminum composite materials, the present invention proposes a preparation method of high-strength interface-bonded beryllium aluminum composite materials by modifying the surface of beryllium powder to form an interface modified layer to coat a beryllium particle precursor.
[0005] The preparation method of the high-strength interface-bonded beryllium aluminum composite material of the present invention is carried out according to the following steps:
[0006] 1. Weighing and surface treatment of raw materials
[0007] Weighing 10% to 50% beryllium metal powder and the remainder of aluminum metal powder as raw materials; cleaning the beryllium metal powder in a cleaning agent containing hydroxyl organic matter to obtain surface sensitized beryllium metal powder;
[0008] 2. Preparation of interface modified layer coated beryllium particle precursor
[0009] The surface-sensitized beryllium metal powder weighed in step 1 is mixed with a liquid silicon-based precursor and subjected to short-time high-energy ball milling; the mixed powder obtained by ball milling is then heat-treated in a vacuum heating furnace under an inert gas, so that the liquid silicon-based precursor is in situ decomposed into a silicon coating that is coated on the surface of the surface-sensitized beryllium metal powder, thereby obtaining an interface-modified layer-coated beryllium particle precursor;
[0010] The heat treatment process is as follows: temperature is 450-550°C and time is 1-5h;
[0011] 3. Preparation of Interface Modified Beryllium-Aluminum Composite Ingot
[0012] The interface modified layer coated beryllium particle precursor obtained in step 2 and the aluminum metal powder weighed in step 1 are dispersed by mechanical ball milling, and then loaded into a steel mold, and cold pressed at a pressure of 50 to 200 MPa to obtain an interface modified beryllium-aluminum preform; then the interface modified beryllium-aluminum preform is placed in a vacuum heating furnace, sintered for 0.5 to 5 hours at a temperature of 530 to 650° C. and a pressure of 50 to 500 MPa, and after cooling, an interface modified beryllium-aluminum composite material ingot is obtained;
[0013] 4. Deformation treatment of high-strength interface-bonded beryllium aluminum composite materials
[0014] The interface-modified beryllium-aluminum composite ingot obtained in step 4 is placed in a steel mold for large plastic deformation treatment to obtain a high-strength interface-bonded beryllium-aluminum composite material;
[0015] The large plastic deformation treatment is an extrusion deformation treatment or a rolling treatment;
[0016] The temperature of the large plastic deformation treatment is 450°C to 550°C, and the deformation ratio is (3 to 30): 1;
[0017] 5. Stress relief annealing treatment
[0018] The high-strength interface-bonded beryllium aluminum composite material obtained in step 5 is subjected to stress relief annealing treatment, and the process is completed;
[0019] The stress relief annealing treatment is performed at a temperature of 300° C. to 360° C. and for a time of 1 to 3 hours.
[0020] Principle and beneficial effects of the present invention:
[0021] 1. The present invention proposes a method for preparing a high-strength interface-bonded beryllium-aluminum composite material, in which a silicon coating is in situ generated on the surface of beryllium metal powder by a liquid silicon-based precursor, thereby avoiding the alloy elements from entering the interior of beryllium and aluminum particles to the greatest extent. The added silicon element is mainly distributed at the beryllium-aluminum interface, thereby ensuring the cleanliness and plasticity of the matrix; the silicon coating forms a high-strength interface bond at the beryllium-aluminum interface, and a beryllium-aluminum metal bridge is formed by the in-situ coating, thereby greatly improving the interface bonding performance.
[0022] 2. The interface modification layer used in the present invention is an interface layer mainly composed of silicon element. The maximum solid solubility of silicon element in aluminum exceeds 12%, and it also has good solubility in beryllium. The silicon interface layer can effectively achieve high-strength bridging of the beryllium-aluminum interface, ensure the interface bonding performance, and solve the key problem of interface cracking of composite materials.
[0023] 3. The present invention uses a liquid silicon-based precursor as a silicon source. The interface layer generated by the liquid precursor relies on the nucleation and growth on the surface of the beryllium metal powder. Therefore, it is easier to form a semi-coherent compatible interface with the beryllium metal powder with a higher degree of matching. The interface bonding strength is higher, which ensures that the beryllium-coating interface does not easily debond during the service of the material, resists the initiation and expansion of cracks from the interface, and is beneficial to improving the mechanical properties of the material.
[0024] 4. The present invention uses hydroxyl-containing organic matter to clean beryllium metal powder. On the one hand, it can wash away oil and impurities on the surface of beryllium metal powder. On the other hand, it can also use polar hydroxyl groups to sensitize the surface of beryllium metal powder, making it more reactive, which is beneficial to coat the interface modification layer on the surface of beryllium metal powder.
[0025] 5. The present invention heat treats the liquid silicon-based precursor and beryllium mixed powder in a vacuum atmosphere furnace, the liquid silicon-based precursor decomposes, silicon is deposited on the surface of the beryllium metal powder, and the remaining components are vacuum extracted in gaseous form, ensuring that the composite material is not contaminated by residual impurities and improving the overall organizational stability.
[0026] 6. The high-strength interface-bonded beryllium aluminum composite material prepared by the present invention has excellent comprehensive performance, with an interface bonding strength exceeding 900MPa, a bending strength greater than 325MPa, a yield strength exceeding 470MPa, a tensile strength exceeding 575MPa, and an elongation exceeding 6.6%;
[0027] 7. The present invention realizes coating and generation of the coating by mechanically dispersing the liquid silicon-based precursor, does not involve complicated chemical processes, does not pollute the environment, has a simple preparation process, has strong repeatability, and is easy to apply in large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the microstructure diagram of the high-strength interface-bonded beryllium aluminum composite material obtained in Example 1. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any reasonable combination of the specific implementation modes.
[0030] Specific implementation method 1: The preparation method of the high-strength interface-bonded beryllium aluminum composite material of this implementation method is carried out according to the following steps:
[0031] 1. Weighing and surface treatment of raw materials
[0032] Weighing 10% to 50% beryllium metal powder and the remainder of aluminum metal powder as raw materials; cleaning the beryllium metal powder in a cleaning agent containing hydroxyl organic matter to obtain surface sensitized beryllium metal powder;
[0033] 2. Preparation of interface modified layer coated beryllium particle precursor
[0034] The surface-sensitized beryllium metal powder weighed in step 1 is mixed with a liquid silicon-based precursor and subjected to short-time high-energy ball milling; the mixed powder obtained by ball milling is then heat-treated in a vacuum heating furnace under an inert gas, so that the liquid silicon-based precursor is in situ decomposed into a silicon coating that is coated on the surface of the surface-sensitized beryllium metal powder, thereby obtaining an interface-modified layer-coated beryllium particle precursor;
[0035] The heat treatment process is as follows: temperature is 450-550°C and time is 1-5h;
[0036] 3. Preparation of Interface Modified Beryllium-Aluminum Composite Ingot
[0037] The interface modified layer coated beryllium particle precursor obtained in step 2 and the aluminum metal powder weighed in step 1 are dispersed by mechanical ball milling, and then loaded into a steel mold, and cold pressed at a pressure of 50 to 200 MPa to obtain an interface modified beryllium-aluminum preform; then the interface modified beryllium-aluminum preform is placed in a vacuum heating furnace, sintered for 0.5 to 5 hours at a temperature of 530 to 650° C. and a pressure of 50 to 500 MPa, and after cooling, an interface modified beryllium-aluminum composite material ingot is obtained;
[0038] 4. Deformation treatment of high-strength interface-bonded beryllium aluminum composite materials
[0039] The interface-modified beryllium-aluminum composite ingot obtained in step 4 is placed in a steel mold for large plastic deformation treatment to obtain a high-strength interface-bonded beryllium-aluminum composite material;
[0040] The large plastic deformation treatment is an extrusion deformation treatment or a rolling treatment;
[0041] The temperature of the large plastic deformation treatment is 450°C to 550°C, and the deformation ratio is (3 to 30): 1;
[0042] 5. Stress relief annealing treatment
[0043] The high-strength interface-bonded beryllium aluminum composite material obtained in step 5 is subjected to stress relief annealing treatment, and the process is completed;
[0044] The stress relief annealing treatment is performed at a temperature of 300° C. to 360° C. and for a time of 1 to 3 hours.
[0045] 1. This embodiment proposes a method for preparing a high-strength interface-bonded beryllium-aluminum composite material, in which a silicon coating is in situ generated on the surface of beryllium metal powder by a liquid silicon-based precursor, and the added silicon element is mainly distributed at the beryllium-aluminum interface, which avoids the alloy elements from entering the beryllium and aluminum particles to the greatest extent, thereby ensuring the cleanliness and plasticity of the matrix; the silicon coating forms a high-strength interface bond at the beryllium-aluminum interface, and a beryllium-aluminum metal bridge is formed by the in-situ coating, which greatly improves the interface bonding performance.
[0046] 2. The interface modification layer used in this embodiment is an interface layer mainly composed of silicon. The maximum solid solubility of silicon in aluminum exceeds 12%, and it also has good solubility in beryllium. The silicon interface layer can effectively achieve high-strength bridging of the beryllium-aluminum interface, ensure the interface bonding performance, and solve the key problem of interface cracking of composite materials.
[0047] 3. This embodiment uses a liquid silicon-based precursor as a silicon source. The interface layer generated by the liquid precursor relies on the nucleation and growth on the surface of the beryllium metal powder. Therefore, it is easier to form a semi-coherent compatible interface with the beryllium metal powder with a higher degree of matching. The interface bonding strength is higher, which ensures that the beryllium-coating interface does not easily debond during the service of the material, resists the initiation and propagation of cracks from the interface, and is beneficial to improving the mechanical properties of the material.
[0048] 4. In this embodiment, beryllium metal powder is cleaned by hydroxyl-containing organic matter. On the one hand, oil and impurities on the surface of beryllium metal powder are washed away. On the other hand, polar hydroxyl groups are used to sensitize the surface of beryllium metal powder, making it more reactive, which is beneficial to coating the surface of beryllium metal powder with an interface modification layer.
[0049] 5. In this embodiment, the liquid silicon-based precursor and beryllium mixed powder are heat-treated in a vacuum atmosphere furnace, the liquid silicon-based precursor is decomposed, silicon is deposited on the surface of the beryllium metal powder, and the remaining components are vacuum-evacuated in gaseous form, ensuring that the composite material is not contaminated by residual impurities and improving the overall organizational stability.
[0050] 6. The high-strength interface-bonded beryllium aluminum composite material prepared in this embodiment has excellent comprehensive performance, with an interface bonding strength exceeding 900 MPa, a bending strength greater than 325 MPa, a yield strength exceeding 470 MPa, a tensile strength exceeding 575 MPa, and an elongation exceeding 6.6%;
[0051] 7. This embodiment realizes coating and generation of the coating by mechanically dispersing the liquid silicon-based precursor, does not involve complex chemical processes, does not pollute the environment, has a simple preparation process, has strong repeatability, and is easy to apply in large-scale production.
[0052] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that: the aluminum metal powder in step 1 is aluminum alloy powder;
[0053] The aluminum alloy powder is composed of one or a combination of Al-Si alloy, Al-Si-Cu alloy, Al-Mg-Si alloy, Al-Cu-Mg alloy, Al-Zn-Cu alloy, Al-Zn-Mg-Cu alloy, Al-Si-Cu-Mg alloy;
[0054] The mass fraction of Si in the Al-Si alloy is 2% to 25%;
[0055] The mass fraction of Si in the Al-Mg-Si alloy is 0.5% to 25%, and the mass fraction of Mg is 0.5% to 50%;
[0056] The mass fraction of Si in the Al-Si-Cu alloy is 0.5% to 25%, and the mass fraction of Cu is 0.5% to 53%;
[0057] The mass fraction of Cu in the Al-Cu-Mg alloy is 0.5% to 53%, and the mass fraction of Mg is 0.5% to 38%;
[0058] The mass fraction of Zn in the Al-Zn-Cu alloy is 0.5% to 55%, and the mass fraction of Cu is 0.5% to 53%;
[0059] The mass fraction of Zn in the Al-Zn-Mg-Cu alloy is 0.5% to 55%, the mass fraction of Mg is 0.5% to 38%, and the mass fraction of Cu is 0.5% to 53%;
[0060] The mass fraction of Si in the Al-Si-Cu-Mg alloy is 0.5% to 25%, the mass fraction of Cu is 0.5% to 53%, and the mass fraction of Mg is 0.5% to 38%.
[0061] Specific implementation method three: This implementation method is different from specific implementation methods one or two in that: the cleaning agent containing hydroxyl organic matter in step one is an aqueous solution of one or more of ethanol, methanol, propanol, phenol, acetone, and formic acid; the mass fraction of the cleaning agent containing hydroxyl organic matter is 50% to 100%.
[0062] Specific implementation method 4: This implementation method is different from any one of specific implementation methods 1 to 3 in that: the cleaning described in step 1 is performed under an ultrasonic environment, the ultrasonic power is 1000 to 5000 W, and the time is 0.5 to 3 hours.
[0063] Specific embodiment 5: This embodiment is different from any one of specific embodiments 1 to 4 in that: the content of the liquid silicon-based precursor in step 2 is 1% to 10% of the mass of the surface-sensitized beryllium metal powder.
[0064] Specific embodiment six: This embodiment differs from any one of specific embodiments one to five in that: the liquid silicon-based precursor in step two is a 30% to 50% SiO2 suspension or a 10% to 30% Si suspension; the mass fraction of SiO2 in the SiO2 suspension is 30% to 50%, and the mass fraction of Si in the Si suspension is 10% to 30%.
[0065] Specific embodiment seven: This embodiment differs from any one of specific embodiments one to six in that: the liquid silicon-based precursor in step two is an ethanol dispersion of a silicon-based precursor; the silicon-based precursor is one or more of polysilane, polysiloxane, polysilazane, silicic acid, metasilicic acid, and disilicate; the mass fraction of the silicon-based precursor in the ethanol dispersion is 50% to 90%.
[0066] Specific implementation eight: This implementation differs from any one of specific implementations one to seven in that the rotation speed of the short-time high-energy ball milling in step two is 300 to 500 r / min, and the time is 10 to 30 min.
[0067] Specific embodiment nine: This embodiment differs from any one of specific embodiments one to eight in that: in step two, the liquid silicon-based precursor is decomposed and heat-treated in a tubular furnace, and the decomposition products are carried away by the air flow flowing in the tubular furnace, so that the silicon coating is coated on the surface of the beryllium metal powder; the air flow rate is 20 to 50 mL / min, and the inert gas used is helium or argon, etc.
[0068] Specific embodiment ten: This embodiment differs from any one of specific embodiments one to nine in that: the mechanical ball milling dispersion process in step three is: the rotation speed is 100 to 250 r / min, and the time is 2 to 10 h; the sintering method in step three is spark plasma sintering.
[0069] Embodiment 1:
[0070] The preparation method of the high-strength interface-bonded beryllium aluminum composite material of this embodiment is carried out by the following steps:
[0071] 1. Weighing and surface treatment of raw materials
[0072] Weighing 50% beryllium metal powder and the rest aluminum metal powder as raw materials; cleaning the beryllium metal powder in a cleaning agent containing hydroxyl organic matter to obtain surface sensitized beryllium metal powder;
[0073] The aluminum metal powder is made of pure aluminum;
[0074] The cleaning agent containing hydroxyl organic matter is an ethanol solution with a mass fraction of 75%;
[0075] The cleaning is carried out in an ultrasonic environment with an ultrasonic power of 2500W and a time of 2h;
[0076] 2. Preparation of interface modified layer coated beryllium particle precursor
[0077] The surface-sensitized beryllium metal powder weighed in step 1 is mixed with a liquid silicon-based precursor and subjected to short-time high-energy ball milling; the mixed powder obtained by ball milling is then heat-treated in a vacuum heating furnace under an inert gas, so that the liquid silicon-based precursor is in situ decomposed into a silicon coating that is coated on the surface of the surface-sensitized beryllium metal powder, thereby obtaining an interface-modified layer-coated beryllium particle precursor;
[0078] The liquid silicon-based precursor content is 2% of the mass of the surface-sensitized beryllium metal powder;
[0079] The liquid silicon-based precursor is an ethanol dispersion of a silicon-based precursor; the silicon-based precursor is polysiloxane and silicic acid, and the volume ratio of polysiloxane to silicic acid is 1:1; the mass fraction of the silicon-based precursor in the ethanol dispersion is 85%.
[0080] The short-time high-energy ball milling has a rotation speed of 400 r / min and a time of 10 min;
[0081] The heat treatment process is as follows: temperature is 500°C and time is 2h;
[0082] The liquid silicon-based precursor is decomposed and heat-treated in a tube furnace, and the decomposition products are taken away by the airflow flowing in the tube furnace, so that the silicon coating is coated on the surface of the beryllium metal powder; the airflow rate is 30 mL / min, and the inert gas used is argon gas;
[0083] 3. Preparation of Interface Modified Beryllium-Aluminum Composite Ingot
[0084] The interface modified layer coated beryllium particle precursor obtained in step 2 and the aluminum metal powder weighed in step 1 are dispersed by mechanical ball milling, and then loaded into a steel mold, and cold pressed at a pressure of 100 MPa to obtain an interface modified beryllium-aluminum preform; then the interface modified beryllium-aluminum preform is placed in a vacuum heating furnace, sintered for 2 hours at a temperature of 580° C. and a pressure of 200 MPa, and after cooling, an interface modified beryllium-aluminum composite material ingot is obtained;
[0085] The mechanical ball milling dispersion process is as follows: the rotation speed is 150r / min and the time is 6h;
[0086] The sintering method is spark plasma sintering;
[0087] 4. Deformation treatment of high-strength interface-bonded beryllium aluminum composite materials
[0088] The interface-modified beryllium-aluminum composite ingot obtained in step 4 is placed in a steel mold for large plastic deformation treatment to obtain a high-strength interface-bonded beryllium-aluminum composite material;
[0089] The large plastic deformation process is an extrusion deformation process;
[0090] The temperature of the large plastic deformation treatment is 450°C and the deformation ratio is 10:1;
[0091] 5. Stress relief annealing treatment
[0092] The high-strength interface-bonded beryllium aluminum composite material obtained in step 5 is subjected to stress relief annealing treatment, and the process is completed;
[0093] The stress relief annealing treatment was performed at a temperature of 340° C. and for a time of 1 h.
[0094] The high-strength interface-bonded beryllium aluminum composite material prepared in this embodiment has excellent comprehensive properties, with an interface bonding strength of 953 MPa, a bending strength of 355 MPa, a yield strength of 501 MPa, a tensile strength of 612 MPa, and an elongation of 7.3%.
[0095] Embodiment 2:
[0096] The preparation method of the high-strength interface-bonded beryllium aluminum composite material of this embodiment is carried out by the following steps:
[0097] 1. Weighing and surface treatment of raw materials
[0098] Weighing 30% beryllium metal powder and the rest aluminum metal powder as raw materials; cleaning the beryllium metal powder in a cleaning agent containing hydroxyl organic matter to obtain surface sensitized beryllium metal powder;
[0099] The aluminum metal powder is made of Al-Cu-Mg alloy, with a Cu content of 4.5% and a Mg content of 1.6%;
[0100] The cleaning agent containing hydroxyl organic matter is acetone;
[0101] The cleaning is carried out in an ultrasonic environment with an ultrasonic power of 2500W and a time of 1h;
[0102] 2. Preparation of interface modified layer coated beryllium particle precursor
[0103] The surface-sensitized beryllium metal powder weighed in step 1 is mixed with a liquid silicon-based precursor and subjected to short-time high-energy ball milling; the mixed powder obtained by ball milling is then heat-treated in a vacuum heating furnace under an inert gas, so that the liquid silicon-based precursor is in situ decomposed into a silicon coating that is coated on the surface of the surface-sensitized beryllium metal powder, thereby obtaining an interface-modified layer-coated beryllium particle precursor;
[0104] The liquid silicon-based precursor content is 5% of the mass of the surface-sensitized beryllium metal powder;
[0105] The liquid silicon-based precursor is a SiO2 suspension; the mass fraction of SiO2 in the SiO2 suspension is 75%;
[0106] The short-time high-energy ball milling has a rotation speed of 300 r / min and a time of 20 min;
[0107] The heat treatment process is as follows: temperature is 450°C and time is 1h;
[0108] The liquid silicon-based precursor is decomposed and heat-treated in a tube furnace, and the decomposition products are taken away by the airflow flowing in the tube furnace, so that the silicon coating is coated on the surface of the beryllium metal powder; the airflow rate is 15 mL / min, and the inert gas used is argon;
[0109] 3. Preparation of Interface Modified Beryllium-Aluminum Composite Ingot
[0110] The interface modified layer coated beryllium particle precursor obtained in step 2 and the aluminum metal powder weighed in step 1 are dispersed by mechanical ball milling, and then loaded into a steel mold, and cold pressed at a pressure of 100 MPa to obtain an interface modified beryllium-aluminum preform; then the interface modified beryllium-aluminum preform is placed in a vacuum heating furnace, sintered for 2 hours at a temperature of 600° C. and a pressure of 150 MPa, and after cooling, an interface modified beryllium-aluminum composite material ingot is obtained;
[0111] The mechanical ball milling dispersion process is as follows: the rotation speed is 150r / min and the time is 3h;
[0112] The sintering method is spark plasma sintering;
[0113] 4. Deformation treatment of high-strength interface-bonded beryllium aluminum composite materials
[0114] The interface-modified beryllium-aluminum composite ingot obtained in step 4 is placed in a steel mold for large plastic deformation treatment to obtain a high-strength interface-bonded beryllium-aluminum composite material;
[0115] The large plastic deformation process is a rolling process;
[0116] The temperature of the large plastic deformation treatment is 550°C and the deformation ratio is 3:1;
[0117] 5. Stress relief annealing treatment
[0118] The high-strength interface-bonded beryllium aluminum composite material obtained in step 5 is subjected to stress relief annealing treatment, and the process is completed;
[0119] The stress relief annealing treatment is performed at a temperature of 355° C. and for a period of 2 hours.
[0120] The high-strength interface-bonded beryllium aluminum composite material prepared in this embodiment has an interface bonding strength of 928 MPa, a bending strength of 330 MPa, a yield strength of 481 MPa, a tensile strength of 585 MPa, and an elongation of 6.9%.
Claims
1. A method for preparing a high-strength interface-bonded beryllium aluminum composite material, characterized in that: The preparation method of the high-strength interface-bonded beryllium aluminum composite material is carried out in the following steps:
1. Weighing and surface treatment of raw materials Weighing 10% to 50% beryllium metal powder and the remainder of aluminum metal powder as raw materials; cleaning the beryllium metal powder in a cleaning agent containing hydroxyl organic matter to obtain surface sensitized beryllium metal powder; 2. Preparation of interface modified layer coated beryllium particle precursor The surface-sensitized beryllium metal powder weighed in step 1 is mixed with a liquid silicon-based precursor and subjected to short-time high-energy ball milling; the mixed powder obtained by ball milling is then heat-treated in a vacuum heating furnace under an inert gas, so that the liquid silicon-based precursor is in situ decomposed into a silicon coating that is coated on the surface of the surface-sensitized beryllium metal powder, thereby obtaining an interface-modified layer-coated beryllium particle precursor; The heat treatment process is as follows: temperature is 450-550°C and time is 1-5h; 3. Preparation of Interface Modified Beryllium-Aluminum Composite Ingot The interface modified layer coated beryllium particle precursor obtained in step 2 and the aluminum metal powder weighed in step 1 are dispersed by mechanical ball milling, and then loaded into a steel mold, and cold pressed at a pressure of 50-200 MPa to obtain an interface modified beryllium-aluminum preform; then the interface modified beryllium-aluminum preform is placed in a vacuum heating furnace, sintered for 0.5-5 h at a temperature of 530-650° C. and a pressure of 50-500 MPa, and after cooling, an interface modified beryllium-aluminum composite material ingot is obtained; 4. Deformation treatment of high-strength interface-bonded beryllium aluminum composite materials The interface-modified beryllium-aluminum composite ingot obtained in step 3 is placed in a steel mold for large plastic deformation treatment to obtain a high-strength interface-bonded beryllium-aluminum composite material; The large plastic deformation treatment is an extrusion deformation treatment or a rolling treatment; The temperature of the large plastic deformation treatment is 450°C to 550°C, and the deformation ratio is (3 to 30): 1; 5. Stress relief annealing treatment The high-strength interface-bonded beryllium aluminum composite material obtained in step 4 is subjected to stress relief annealing treatment, and the process is completed; The stress relief annealing treatment is performed at a temperature of 300° C. to 360° C. and for a time of 1 to 3 hours.
2. The method for preparing the high-strength interface-bonded beryllium aluminum composite material according to claim 1, characterized in that: The cleaning agent for the hydroxyl-containing organic matter in step 1 is an aqueous solution of one or more of ethanol, methanol, propanol, phenol, and formic acid; The mass fraction of the cleaning agent containing hydroxyl organic matter is 50-100%.
3. The method for preparing the high-strength interface-bonded beryllium aluminum composite material according to claim 1, characterized in that: The cleaning in step 1 is carried out in an ultrasonic environment with an ultrasonic power of 1000-5000W and a time of 0.5-3h.
4. The method for preparing the high-strength interface-bonded beryllium aluminum composite material according to claim 1, characterized in that: The content of the liquid silicon-based precursor in step 2 is 1% to 10% of the mass of the surface-sensitized beryllium metal powder.
5. The method for preparing the high-strength interface-bonded beryllium aluminum composite material according to claim 1, characterized in that: The liquid silicon-based precursor in step 2 is a SiO2 suspension or a Si suspension; The mass fraction of SiO2 in the SiO2 suspension is 30% to 50%, and the mass fraction of Si in the Si suspension is 10% to 30%.
6. The method for preparing the high-strength interface-bonded beryllium aluminum composite material according to claim 1, characterized in that: The liquid silicon-based precursor in step 2 is an ethanol dispersion of a silicon-based precursor; The silicon-based precursor is one or more of polysilane, polysiloxane, polysilazane, silicic acid, metasilicic acid, and disilicate; The mass fraction of the silicon-based precursor in the ethanol dispersion is 50% to 90%.
7. The method for preparing the high-strength interface-bonded beryllium aluminum composite material according to claim 1, characterized in that: The rotation speed of the short-time high-energy ball milling in step 2 is 300-500 r / min, and the time is 10-30 min.
8. The method for preparing the high-strength interface-bonded beryllium aluminum composite material according to claim 1, characterized in that: In step 2, the liquid silicon-based precursor is decomposed and heat-treated in a tube furnace; the gas flow rate is 20-50 mL / min, and the inert gas used is helium or argon.
9. The method for preparing the high-strength interface-bonded beryllium aluminum composite material according to claim 1, characterized in that: The mechanical ball milling dispersion process in step 3 is as follows: the rotation speed is 100-250 r / min, and the time is 2-10 h; The sintering method in step three is spark plasma sintering.