Modified rubber powder and preparation method thereof, composition for non-curing waterproof coating, high-viscosity non-curing waterproof coating and preparation method thereof
Through the preparation of modified rubber powder and the design of composition, the shortcomings of non-cured waterproof coatings in terms of heat resistance, self-healing and bonding properties are solved, and the excellent performance and cost-effectiveness of high-viscosity coatings are achieved, and suitable for low temperatures Waterproof application under conditions.
Patent Information
- Application Number
- CN202410274459.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-03-11
AI Technical Summary
Existing non-curing waterproof coatings have shortcomings in heat resistance, self-healing and bonding properties, especially under low temperature conditions.
By preparing the modified rubber powder, the rubber powder is soaked using specific solutes in the first and second solutions to prepare the modified rubber powder and combine it with asphalt, softened oil, thermoplastic elastomer and filler. Form a high viscosity non-curing waterproof coating.
The excellent heat resistance, low temperature flexibility and bonding properties of high viscosity non-curing waterproof coatings are achieved, reducing costs and improving the recycling and reuse efficiency of used tires.
Smart Images

Figure CN118240288B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of waterproof coatings, and in particular to modified rubber powder and a preparation method thereof, a composition for non-curing waterproof coatings, a high-viscosity non-curing waterproof coating and a preparation method thereof. Background Art
[0002] Non-curing waterproof coatings have the characteristics of good creep resistance, strong self-healing ability and excellent bonding performance. They are widely used in various waterproof projects and have become one of the fastest-growing waterproof materials in the waterproof industry.
[0003] However, traditional non-curing waterproof coatings are mainly composed of rubber and asphalt. Among them, rubber components can improve the high and low temperature performance of the material, but they are relatively expensive, and the high amount of addition has a great impact on the viscosity and surface adhesion of the material; secondly, asphalt has defects such as low softening point and poor low temperature resistance, which makes it difficult for existing non-curing waterproof coatings to balance heat resistance, surface adhesion and self-healing properties.
[0004] In addition to using styrene-butadiene rubber polymer modifiers, the existing technology mainly uses resin and wax powder to improve the high temperature resistance of the material, but it will cause the material to deteriorate at low temperatures. At the same time, the resin and wax powder are easy to precipitate, resulting in a decrease in the surface viscosity and self-healing property of the material. Rubber powder is also used for modification, but due to the high degree of vulcanization, the rubber powder absorbs oil severely during the swelling process, resulting in a significant increase in product viscosity and a significant decrease in surface viscosity. In addition, the particles are larger after swelling, making the material surface rough and reducing the self-healing property.
[0005] CN115124925A discloses a non-curing rubber asphalt coating, comprising the following components: 70# asphalt, 200# asphalt, styrene-butadiene rubber (SBR), compound rubber powder, wherein the compound rubber powder is composed of rubber wheel rubber powder (taken from rubber wheels or pulleys of flatbed carts), tire rubber powder and sole rubber powder. In this scheme, the rubber powder is not modified, and the prepared non-curing rubber asphalt coating has insufficient self-healing property and surface viscosity at low temperature, and is limited in use in some seasons and under low temperature conditions.
[0006] CN111171785A discloses a cold-bonded non-curing modified asphalt waterproof material, the raw materials of which include petroleum asphalt, improved asphalt, operating oil, heat-resistant reinforcing material, reinforcing bonding material, viscosity-controlling material, fluidity-blocking mixture, rubber powder, improved water-based material, amphiphilic viscosity enhancer, and reinforcing strength material; the rubber powder is recycled rubber powder. In this scheme, the rubber powder is not modified, and the prepared waterproof material has insufficient self-healing property and surface viscosity at low temperature, and is limited in use in some seasons and under low temperature conditions.
[0007] Therefore, there is an urgent need to provide a non-curing rubber asphalt waterproof coating with good heat resistance, strong self-healing ability and excellent bonding performance. Summary of the invention
[0008] The purpose of the present invention is to overcome the problems of poor heat resistance, poor self-healing property and poor adhesion of the non-curing waterproof coating in the prior art.
[0009] In order to achieve the above object, one aspect of the present invention provides a method for preparing modified rubber powder, the method comprising:
[0010] (1) Rubber powder is subjected to a first immersion treatment in a first solution to obtain rubber powder I; the first solution contains a solute I; the solute I has a structure shown in formula (I):
[0011]
[0012] Wherein, in formula (I), R 1 and R 2 are each independently methyl or ethyl, A - Selected from F - , Cl - Br - ,I - At least one of; and n is an integer from 12 to 20;
[0013] (2) subjecting the rubber powder I to a second immersion treatment in a second solution to obtain a modified rubber powder; the second solution contains a solute II, and the solute II has a structure represented by formula (II):
[0014]
[0015] Wherein, in formula (II), B - Selected from F - , Cl - Br - ,I - At least one of;
[0016] One of R1, R2 and R3 is a hydroxyethyl group, and the other two are each independently selected from one of C1-C6 alkyl groups; or,
[0017] R1, R2 and R3 are each independently selected from one of C1-C6 alkyl groups.
[0018] The second aspect of the present invention provides modified rubber powder prepared by the method described in the first aspect.
[0019] The third aspect of the present invention provides a composition for a non-curing waterproof coating, the composition comprising asphalt, softening oil, thermoplastic elastomer, filler, modified rubber powder, and the composition may further optionally contain wax powder and / or resin;
[0020] Relative to 50 parts by weight of the asphalt, the content of the softening oil is 5-10 parts by weight, the content of the thermoplastic elastomer is 7-13 parts by weight, the content of the filler is 15-30 parts by weight, the content of the modified rubber powder is 3-8 parts by weight, the content of the wax powder is 0-10 parts by weight, and the content of the resin is 0-10 parts by weight;
[0021] The modified rubber powder is the modified rubber powder described in the second aspect above.
[0022] The fourth aspect of the present invention provides a method for preparing a high-viscosity non-curing waterproof coating, the method comprising: mixing and contacting the components in the non-curing waterproof coating composition described in the third aspect to obtain a high-viscosity non-curing waterproof coating.
[0023] The fifth aspect of the present invention provides a high-viscosity non-curing waterproof coating prepared by the method described in the fourth aspect.
[0024] Through the above technical solution, the present invention has at least the following advantages:
[0025] (1) The present invention uses modified rubber as the raw material of the waterproof coating, which has lower cost.
[0026] (2) The high-viscosity non-curing waterproof coating provided by the present invention has excellent heat resistance, low-temperature flexibility, self-healing and bonding properties.
[0027] (3) The present invention uses tire rubber powder as raw material, which can improve the recycling efficiency of waste tires and conform to the concept of green development. DETAILED DESCRIPTION
[0028] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0029] In the present invention, "C1-C6 alkyl" means a straight-chain or branched alkyl group having a total carbon atom number of 1-6, for example, a straight-chain alkyl group having a total carbon atom number of 1, 2, 3, 4, 5 or 6, or a branched alkyl group having a total carbon atom number of 3, 4, 5 or 6, including but not limited to methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, n-hexyl, etc.
[0030] In the present invention, “n is an integer of 12-20” means that n includes 12, 13, 14, 15, 16, 17 or 18. Similarly, “n is an integer of 12-16” means that n includes 12, 13, 14, 15 or 16.
[0031] As mentioned above, one aspect of the present invention provides a method for preparing modified rubber powder, the method comprising:
[0032] (1) Rubber powder is subjected to a first immersion treatment in a first solution to obtain rubber powder I; the first solution contains a solute I; the solute I has a structure shown in formula (I):
[0033]
[0034] Wherein, in formula (I), R 1 and R 2 are each independently methyl or ethyl, A - Selected from F - , Cl - Br - ,I - At least one of; and n is an integer from 12 to 20;
[0035] (2) subjecting the rubber powder I to a second immersion treatment in a second solution to obtain a modified rubber powder; the second solution contains a solute II, and the solute II has a structure represented by formula (II):
[0036]
[0037] Wherein, in formula (II), B - Selected from F - , Cl - Br - ,I - At least one of;
[0038] One of R1, R2 and R3 is a hydroxyethyl group, and the other two are each independently selected from one of C1-C6 alkyl groups; or,
[0039] R1, R2 and R3 are each independently selected from one of C1-C6 alkyl groups.
[0040] Preferably, the mass ratio of the rubber powder, the solute I and the solute II is 10:0.5-2:8-12.
[0041] Preferably, in step (1), in formula (I), R 1 and R 2 are each independently methyl or ethyl, A - Selected from F - , Cl- Br - ,I - At least one of; and n is an integer from 12 to 16.
[0042] More preferably, in step (1), the solute I is selected from at least one of hexadecyl dimethyl benzyl ammonium chloride, hexadecyl diethyl benzyl ammonium bromide, hexadecyl diethyl benzyl ammonium iodide, octadecyl dimethyl benzyl ammonium chloride and tetradecyl dimethyl benzyl ammonium chloride. The inventors of the present invention have found that in this preferred case, the non-curing waterproof coating provided by the present invention has better heat resistance, self-healing properties and bonding properties.
[0043] Preferably, in step (1), the average particle size of the rubber powder is 100-400 μm.
[0044] More preferably, the rubber powder is tire rubber powder.
[0045] Preferably, in step (1), the concentration of solute I in the first solution is 2-10 wt %.
[0046] More preferably, in step (1), the solvent of the first solution is ethanol.
[0047] Preferably, in step (1), the conditions of the first immersion treatment include: a time of 48-96 hours.
[0048] According to a preferred embodiment, the method further comprises, in step (1), filtering and separating the obtained substance I after the first soaking treatment to obtain the rubber powder I. The present invention has no special requirements for the specific operation of the filtering and separation, and the operation known in the art can be used.
[0049] Preferably, in step (2), the solute II is selected from at least one of (2-hydroxyethyl)trimethylammonium chloride, (2-hydroxyethyl)trimethylammonium bromide, (2-hydroxyethyl)trimethylammonium iodide and (2-hydroxyethyl)triethylammonium chloride.
[0050] Preferably, in step (2), the concentration of solute II in the second solution is 8-15 wt %.
[0051] More preferably, in step (2), the solvent of the second solution is water.
[0052] Preferably, in step (2), the conditions of the second immersion treatment include: a time of 0.5-48 hours.
[0053] According to a particularly preferred embodiment, the method further comprises, in step (2), filtering, washing and drying the obtained substance II in sequence after the second immersion treatment to obtain the modified rubber powder.
[0054] It should be noted that the present invention has no special requirements for the filtering and washing, and operations known in the art can be used. For example, ethanol can be used for multiple washings before filtering.
[0055] In the present invention, there is no special requirement for the temperature of the first immersion treatment in step (1) and the second immersion treatment in step (2), and any temperature known in the art may be used. However, in order to obtain a high-viscosity non-curing waterproof coating with better heat resistance, the present invention preferably adopts the temperature of the first immersion treatment and the temperature of the second immersion treatment to be independently 10-60°C.
[0056] Preferably, the drying conditions include: temperature of 105-120° C. and time of 1-2 h.
[0057] As mentioned above, the second aspect of the present invention provides modified rubber powder prepared by the method described in the second aspect.
[0058] As mentioned above, the third aspect of the present invention provides a composition for a non-curing waterproof coating, the composition comprising asphalt, softening oil, thermoplastic elastomer, filler, modified rubber powder, and the composition may further optionally contain wax powder and / or resin;
[0059] Relative to 50 parts by weight of the asphalt, the content of the softening oil is 5-10 parts by weight, the content of the thermoplastic elastomer is 7-13 parts by weight, the content of the filler is 15-30 parts by weight, the content of the modified rubber powder is 3-8 parts by weight, the content of the wax powder is 0-10 parts by weight, and the content of the resin is 0-10 parts by weight;
[0060] The modified rubber powder is the modified rubber powder described in the second aspect above.
[0061] Preferably, the asphalt is selected from at least one of 150# asphalt, 200# asphalt and 300# asphalt. The inventors of the present invention have found that in this preferred embodiment, the high-viscosity non-curing waterproof coating provided by the present invention has better waterproof performance.
[0062] Preferably, the softening oil has a viscosity of 8-15 mPa.s at 100°C, a flash point ≥210°C, a pour point <-20°C, and an aniline point ≤120°C.
[0063] More preferably, the softening oil is selected from at least one of aromatic oil, base oil, naphthenic oil and reduced oil. The inventors of the present invention have found that in this preferred case, the high-viscosity non-curing waterproof coating provided by the present invention has better adhesion and is easier to construct.
[0064] Preferably, the volatile matter of the thermoplastic elastomer is ≤0.8wt%, and the melt flow rate at 200°C and 5Kg is 1-15g / 10min.
[0065] More preferably, the thermoplastic elastomer is at least one selected from butadiene-styrene-butadiene triblock copolymer, styrene-butadiene rubber, hydrogenated styrene-butadiene block copolymer and butadiene-isoprene-butadiene triblock copolymer.
[0066] Further preferably, the thermoplastic elastomer is a combination of butadiene-styrene-butadiene triblock copolymer and styrene-butadiene rubber in a content mass ratio of 1:1-4. The inventors of the present invention have found that in this preferred case, the high-viscosity non-curing waterproof coating provided by the present invention has better high and low temperature performance and elongation.
[0067] Preferably, the filler is selected from at least one of talc, heavy calcium, montmorillonite, kaolin and metakaolin. More preferably, the average particle size of the filler is 15-75 μm.
[0068] Preferably, the wax powder has a viscosity of 100-500 mPa.s at 130° C., a softening point of 100-120° C., and a number average molecular weight of 1200-3000.
[0069] Preferably, the resin has a number average molecular weight of 2000-5000, a relative density of 0.95-1.08, and a softening point of 80-140° C. More preferably, the resin is selected from at least one of C5 hydrogenated petroleum resin, C9 hydrogenated petroleum resin, C5 / C9 copolymerized petroleum resin, and cycloaliphatic resin.
[0070] As mentioned above, the fourth aspect of the present invention provides a method for preparing a high-viscosity non-curing waterproof coating, the method comprising: mixing and contacting the components in the non-curing waterproof coating composition described in the third aspect to obtain a high-viscosity non-curing waterproof coating.
[0071] It should be noted that the present invention has no special requirements for the specific method of the mixing and contacting, and can be carried out by methods known in the art. For example, asphalt, softening oil, thermoplastic elastomer, filler, modified rubber powder, and optionally wax powder and / or resin can be mixed and contacted. However, in order to obtain a high-viscosity non-curing waterproof coating with better heat resistance, low-temperature flexibility and self-healing performance, the present invention preferably adopts the preferred specific embodiment described below to carry out the mixing and contacting.
[0072] According to a preferred embodiment, the mixed contact operation includes:
[0073] S1: first stirring and mixing asphalt, softening oil, thermoplastic elastomer and modified rubber powder to obtain a mixture I;
[0074] S2: performing a second stirring mixing of the mixture I and the components in combination B to obtain the high-viscosity non-curing waterproof coating; the combination B contains fillers, and the combination B optionally further contains wax powder and / or resin.
[0075] Preferably, the first stirring and mixing conditions include: temperature of 150-190° C. and time of 2-3 h.
[0076] Preferably, the second stirring and mixing conditions include: temperature of 130-150° C. and time of 1-2 h.
[0077] According to a particularly preferred embodiment, the method further comprises, in step S1, preheating the asphalt and softened oil to 150-160°C, adding the thermoplastic elastomer and modified rubber powder to the preheated mixture of asphalt and softened oil for a first stirring and mixing to obtain mixture I.
[0078] It should be noted that the first stirring and mixing time is counted from the time when the thermoplastic elastomer and modified rubber powder are added to the preheated mixture of asphalt and softened oil, that is, the time for preheating the asphalt and softened oil is not included.
[0079] Preferably, relative to 50 parts by weight of the asphalt, the amount of the softening oil is 5-10 parts by weight, the amount of the thermoplastic elastomer is 7-13 parts by weight, the amount of the filler is 15-30 parts by weight, the amount of the modified rubber powder is 3-8 parts by weight, the amount of the wax powder is 0-10 parts by weight, and the amount of the resin is 0-10 parts by weight.
[0080] In the present invention, there is no special requirement for the stirring rates of the first stirring and mixing in step S1 and the second stirring and mixing in step S2, and any stirring rate known in the art may be adopted.
[0081] As mentioned above, the fifth aspect of the present invention provides a high-viscosity non-curing waterproof coating prepared by the method described in the fourth aspect.
[0082] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, all raw materials and instruments used are commercially available, and the specific sources of the raw materials are shown in Table 1.
[0083] Table 1
[0084]
[0085]
[0086] The preparation example of the present invention is used to prepare modified rubber powder.
[0087] Preparation Example 1
[0088] (1) The rubber powder is subjected to a first immersion treatment in a first solution and then filtered and separated to obtain rubber powder I; the solvent of the first solution is ethanol, and the conditions of the first immersion treatment are: time is 72 hours, and temperature is 25° C.
[0089] (2) After the rubber powder I is subjected to a second immersion treatment in a second solution, the obtained substance II is washed three times with ethanol, filtered and dried to obtain a modified rubber powder F1. The solvent of the second solution is water, and the conditions for the second immersion treatment are: time for 24 hours, temperature for 25° C., and the conditions for drying include: temperature for 105° C., time for 2 hours.
[0090] Unless otherwise specified, the remaining preparation examples were carried out in accordance with the method of Preparation Example 1, except that the types of substances, concentrations and process parameters used in each preparation example were different. For the types of substances and concentrations, see Table 2.
[0091] Table 2
[0092]
[0093]
[0094] Comparative Preparation Example 1
[0095] This comparative preparation example is carried out in accordance with the method of Preparation Example 1, except that in step (1), this comparative preparation example uses an equal mass of solute I-3 to replace the solute I-1 in Preparation Example 1 to prepare modified rubber powder DF1.
[0096] Comparative Preparation Example 2
[0097] This comparative preparation example is carried out by referring to the method of Preparation Example 1, except that in step (2), this comparative preparation example uses an equal mass of solute II-4 to replace the solute I-1 in Preparation Example 1 to prepare modified rubber powder DF2.
[0098] The embodiments of the present invention are used to prepare a high-viscosity non-curing waterproof coating. The amounts of raw materials in the following examples are all parts by weight unless otherwise specified, and each part by weight represents 10 g.
[0099] Example 1
[0100] S1: After preheating the asphalt and softening oil to 160° C., adding the thermoplastic elastomer and the modified rubber powder to the preheated mixture of the asphalt and softening oil for a first stirring and mixing, to obtain a mixture I;
[0101] S2: The mixture I is mixed with the components in the combination B for a second time to obtain the high-viscosity non-curing waterproof coating.
[0102] The material types and parameters of this example are shown in Table 3.
[0103] Unless otherwise specified, the remaining examples are carried out in accordance with the method of Example 1, except that the types of substances, amounts and process parameters used in each example are different, see Table 3 for details.
[0104] Table 3
[0105]
[0106]
[0107] Example 4
[0108] This embodiment is carried out in accordance with the method of embodiment 1, except that in step S1, this embodiment uses modified rubber powder F4 in equal parts by weight to replace the modified rubber powder F1 in embodiment 1.
[0109] Example 5
[0110] This embodiment is carried out in accordance with the method of embodiment 1, except that in step S1, this embodiment uses modified rubber powder F5 in equal parts by weight to replace the modified rubber powder F1 in embodiment 1.
[0111] Example 6
[0112] This example is carried out by referring to the method of Example 1, except that the amounts of raw materials used are different. The amount of thermoplastic elastomer I is adjusted to 5 parts by weight, the amount of thermoplastic elastomer II is adjusted to 4 parts by weight, and the amounts of other raw materials are the same as in Example 1.
[0113] Comparative Example 1
[0114] This comparative example was carried out in accordance with the method of Example 1, except that in step S1, the modified rubber powder F1 in Example 1 was replaced by an equal weight portion of modified rubber powder DF1.
[0115] Comparative Example 2
[0116] This comparative example was carried out in accordance with the method of Example 1, except that in step S1, the modified rubber powder DF2 in equal parts by weight was used to replace the modified rubber powder F1 in Example 1.
[0117] Comparative Example 3
[0118] This comparative example was carried out in accordance with the method of Example 1, except that in step S1, the modified rubber powder F1 in Example 1 was replaced by rubber powder in equal parts by weight.
[0119] Comparative Example 4
[0120] This comparative example was carried out in accordance with the method of Example 2, except that in step S1, the modified rubber powder F2 in Example 2 was replaced by rubber powder in equal parts by weight.
[0121] Comparative Example 5
[0122] This comparative example was carried out by referring to the method of Example 1, except that the amounts of raw materials used were different. In this comparative example, no modified rubber powder was added, and the amount of thermoplastic elastomer II was adjusted to 13 parts by weight. The amounts of other raw materials used were the same as in Example 1.
[0123] Comparative Example 6
[0124] This comparative example was carried out in accordance with the method of Example 1, except that the amounts of raw materials used were different. In this comparative example, no modified rubber powder was added, and the amount of wax powder was adjusted to 11 parts by weight. The amounts of the remaining raw materials were the same as in Example 1.
[0125] Comparative Example 7
[0126] This comparative example was carried out in accordance with the method of Example 1, except that the amount of raw materials used was different. In this comparative example, no modified rubber powder was added, and resin was added, and the amount of resin was adjusted to 8 parts by weight. The amounts of other raw materials were the same as in Example 1.
[0127] Comparative Example 8
[0128] This comparative example was carried out with reference to the method of Example 1, except that the amounts of raw materials used were different. In this comparative example, no modified rubber powder was added, and the amount of filler was adjusted to 28 parts by weight. The amounts of other raw materials used were the same as in Example 1.
[0129] Test Case
[0130] Referring to the standard J / CT 2428-2017, the high viscosity non-curing waterproof coating prepared in the above example was subjected to relevant performance tests. The experimental results are shown in Table 4.
[0131] Table 4
[0132]
[0133] It can be seen from the results in Table 4 that the high-viscosity non-curing waterproof coating provided by the present invention has better heat resistance, low-temperature flexibility, self-healing property and bonding performance.
[0134] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing modified rubber powder, characterized in that: The method includes: (1) Rubber powder is subjected to a first immersion treatment in a first solution to obtain rubber powder I; the first solution contains a solute I; the solute I has a structure shown in formula (I): Wherein, in formula (I), R 1 and R 2 are each independently methyl or ethyl, A - Selected from F - , Cl - Br - ,I - At least one of; and n is an integer from 12 to 20; (2) subjecting the rubber powder I to a second immersion treatment in a second solution to obtain a modified rubber powder; the second solution contains a solute II, and the solute II is selected from at least one of (2-hydroxyethyl)trimethylammonium chloride, (2-hydroxyethyl)trimethylammonium bromide, (2-hydroxyethyl)trimethylammonium iodide, and (2-hydroxyethyl)triethylammonium chloride.
2. The method according to claim 1, wherein: The mass ratio of the rubber powder, the solute I and the solute II is 10:0.5-2:8-12.
3. The method according to claim 1 or 2, wherein: In step (1), in formula (I), R 1 and R 2 Each independently is methyl or ethyl, A- is selected from F-, Cl-, Br - , I-; and n is an integer from 12 to 16.
4. The method according to claim 1 or 2, wherein: In step (1), the average particle size of the rubber powder is 100-400 μm; and the concentration of the solute I in the first solution is 2-10 wt %.
5. The method according to claim 1 or 2, wherein: In step (2), the concentration of solute II in the second solution is 8-15 wt %.
6. Modified rubber powder prepared by the method described in any one of claims 1 to 5.
7. A composition for non-curing waterproof coating, characterized in that: The composition contains asphalt, softening oil, thermoplastic elastomer, filler, modified rubber powder, and optionally contains wax powder and / or resin; Relative to 50 parts by weight of the asphalt, the content of the softening oil is 5-10 parts by weight, the content of the thermoplastic elastomer is 7-13 parts by weight, the content of the filler is 15-30 parts by weight, the content of the modified rubber powder is 3-8 parts by weight, the content of the wax powder is 0-10 parts by weight, and the content of the resin is 0-10 parts by weight; The modified rubber powder is the modified rubber powder described in claim 6.
8. The composition according to claim 7, wherein The volatile matter of the thermoplastic elastomer is ≤0.8wt%, and the melt flow rate is 1-15g / 10min under the conditions of 200°C and 5Kg.
9. The composition according to claim 8, wherein The thermoplastic elastomer is a combination of butadiene-styrene-butadiene triblock copolymer and styrene-butadiene rubber in a content mass ratio of 1:1-4.
10. A method for preparing a high-viscosity non-curing waterproof coating, characterized in that: The method comprises: mixing and contacting the components in the non-curing waterproof coating composition according to any one of claims 7 to 9 to obtain a high-viscosity non-curing waterproof coating.
11. The method according to claim 10, wherein: The mixed contact operation includes: S1: first stirring and mixing asphalt, softening oil, thermoplastic elastomer and modified rubber powder to obtain a mixture I; S2: performing a second stirring mixing of the mixture I and the components in combination B to obtain the high-viscosity non-curing waterproof coating; the combination B contains fillers, and the combination B optionally further contains wax powder and / or resin.
12. The method according to claim 11, wherein: The first stirring and mixing conditions include: temperature of 150-190° C. and time of 2-3 h.
13. The method according to claim 11, wherein: The second stirring and mixing conditions include: temperature of 130-150° C. and time of 1-2 h.
14. A high-viscosity non-curing waterproof coating prepared by the method according to any one of claims 10 to 13.
Citation Information
Patent Citations
Cold-bonded non-cured modified asphalt waterproof material and preparation method thereof, and waterproof coiled material containing cold-bonded non-cured modified asphalt waterproof material
CN111171785A
Non-cured rubber asphalt coating and preparation method thereof
CN115124925A
Method for preparing emulsified rubber asphalt
CN103289105A
Modified asphalt composition particle and preparation method thereof
CN105585862A
Root-resistant water-based spraying and non-cured rubber asphalt waterproof coating
CN107446501A