A super soft silicone sealant for road and bridge engineering joints

By adding specific softeners and crosslinking agents to the silicone glue, the elongation and elastic recovery rate of breaking are improved, and the toughness and elasticity of ketoxime silicone glue is solved, achieving better mechanical properties and long-term Time-elastic deformation capability, suitable for road joint potting, improving safety and durability.

CN118240524BActive Publication Date: 2024-11-12FOSHAN PULIDA TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410516083.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-27
Publication Date
2024-11-12
Estimated Expiration
2044-04-27

AI Technical Summary

Technical Problem

The existing ketoxime silicone glue has a decrease in toughness and elasticity after a long period of time, which is prone to detachment of the glue interface and cracking of the glue joint due to road vibration or temperature difference, which poses safety hazards.

Method used

Ultra-soft road and bridge engineering joints including α,ω-dihydroxypolydimethylsiloxane, dimethylsiloxane, reinforcement filler, deketoxime crosslinker, silane coupling agent, catalyst and softener Potting silicone formula, by adding softeners such as fatty alcohol polyoxyethylene ether or polyethylene glycol oleate, the elongation and elastic recovery of silicone glue is enhanced, and its mechanical properties and elastic deformation ability are enhanced.

Benefits of technology

It effectively improves the toughness and elasticity of silicone glue, prevents bonding failure caused by road vibration, is suitable for bonding environments of complex substrates, and improves the durability and safety of road joint potting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a super-soft road and bridge engineering joint potting silica gel, and relates to the technical field of silicone glue. A super-soft road and bridge engineering joint potting silica gel comprises the following raw materials by weight: 45-60 parts of α, ω-dihydroxy polydimethylsiloxane, 25-40 parts of dimethyl silicone oil, 10-40 parts of reinforcing filler, 4-7 parts of deketoxime cross-linking agent, 0.8-1.6 parts of silane coupling agent, 0.03-0.05 parts of catalyst, 0.3-1 parts of softener, wherein the softener is selected from polyethylene glycol oleate or fatty alcohol polyoxyethylene ether. After adding any one of the softeners of fatty alcohol polyoxyethylene ether, polyethylene glycol oleate or polypropylene glycol oleate, it is not only beneficial to improve the elongation at break and elastic recovery rate of silicone glue, so that silicone glue has good mechanical properties, but also silicone glue can still have good elastic deformation ability and elastic recovery ability after a long time, which is beneficial to prevent the occurrence of adhesive failure caused by long-term vibration of the highway.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicone adhesive, in particular to a super-soft road and bridge engineering joint potting silicone adhesive. Background Art

[0002] With the trend of prefabrication, high-rise, high-end interior and exterior decoration and renovation of the construction industry, and the large-scale adoption of large-scale frame hanging plate structures, the construction industry has higher and higher requirements for the aging resistance and bonding performance of sealing materials. Silicone sealants are gradually being widely used in decoration, waterproofing, glass installation and curtain wall structure bonding due to their advantages such as resistance to weather aging, water erosion and excellent adhesion to glass.

[0003] At present, most of the silicone adhesives used for sealing highway joints on the market are neutral ketoxime silicone adhesives. Compared with the neutral alcohol silicone adhesives, ketoxime silicone adhesives have better bonding performance and curing efficiency for different substrates, and can fully bond reinforced concrete in highway joints. However, the toughness and elasticity of ketoxime silicone adhesives are worse than those of general alcohol silicone adhesives. As time goes by, ketoxime silicone adhesives will gradually harden, and the colloid will also lose its toughness and elasticity, making it more likely to cause the bonding interface to detach or the glue joint to crack due to long-term vibration of the highway or changes in the temperature difference between day and night, and form bonding failure, which poses certain safety hazards. Summary of the invention

[0004] In order to improve the toughness and elasticity of ketoxime silicone adhesive, so that ketoxime silicone adhesive can still maintain good elastic deformation ability and elastic recovery ability after a long time, and prevent the occurrence of adhesive failure due to road vibration, the present application provides a super soft road and bridge engineering joint sealing silicone.

[0005] In the first aspect, the present application provides a super soft road and bridge engineering joint potting silica gel, which adopts the following technical solution:

[0006] A super-soft road and bridge engineering joint potting silica gel comprises the following raw materials in parts by weight:

[0007] α,ω-dihydroxy polydimethylsiloxane: 45-60 parts;

[0008] Dimethyl silicone oil: 25-40 parts;

[0009] Reinforcing filler: 10-40 parts;

[0010] Deketoxime type cross-linking agent: 4-7 parts;

[0011] Silane coupling agent: 0.8-1.6 parts;

[0012] Catalyst: 0.03-0.05 parts;

[0013] Softener: 0.3-1 part;

[0014] Wherein, the softener is selected from one of fatty alcohol polyoxyethylene ether and polyethylene glycol oleate.

[0015] By adopting the above technical scheme, after adding any one of the softeners of fatty alcohol polyoxyethylene ether or polyethylene glycol oleate, the elongation at break and elastic recovery rate of silicone adhesive can be effectively improved, so that the toughness and elasticity of ketoxime silicone adhesive after curing are close to those of alcohol silicone adhesive, and it has good mechanical properties, and can still have good elastic deformation ability and elastic recovery ability after a long time, which is beneficial to prevent the occurrence of adhesive failure due to long-term vibration of the road, and is more suitable for the encapsulation project of highway joints.

[0016] Optionally, the softener is fatty alcohol polyoxyethylene ether, specifically any one or more of AEO-5, AEO-6, AEO-9, and AEO-10 ​​are mixed.

[0017] By adopting the above technical scheme, the lipophilic long-chain aliphatic segment and the hygroscopic EO segment in the fatty alcohol polyoxyethylene ether are not only beneficial to improving the elasticity and toughness of the silicone glue after curing, but also beneficial to increasing the overall curing speed of the silicone glue.

[0018] Optionally, the softener is polyethylene glycol oleate or polypropylene glycol oleate, specifically any one of PEG-400MO, PEG-400DO, PEG-600MO, PEG-600DO, PPG-400MO, PPG-400DO, PPG-600MO, and PPG-600DO.

[0019] By adopting the above technical scheme, polyethylene glycol oleate or polypropylene glycol oleate both have hygroscopic EO or PO segments and lipophilic long-chain oleate segments. The oleate segments can further improve the cohesive force of the colloid itself, which is beneficial to improving the elasticity and toughness of the silicone glue after curing, and the hygroscopicity of the EO or PO segments is also beneficial to improving the overall curing speed of the silicone glue.

[0020] Optionally, the deketoxime type cross-linking agent is selected from methyltributylacetoximine silane or vinyltributylacetoximine silane.

[0021] By adopting the above technical scheme, methyl tributylacetonate oxime silane or vinyl tributylacetonate oxime silane has a strong cross-linking ability. Under the action of a catalyst, methyl tributylacetonate oxime silane or vinyl tributylacetonate oxime silane can be rapidly hydrolyzed and the adhesive can be reacted and cured, which is beneficial to improving the overall curing speed of the silicone adhesive and enabling it to cure rapidly.

[0022] Optionally, the deketoxime type crosslinking agent is methyltributylidene oxime silane, and the softener is PPG-600DO.

[0023] By adopting the above technical solution, the overall curing speed of silicone adhesive is more stable, and it can maintain relatively excellent elongation at break and elastic recovery rate, which is conducive to the preparation of deketoxime silicone adhesive with excellent comprehensive performance.

[0024] Optionally, the silane coupling agent is a mixture of two silane coupling agents, KH-550 and KH-792, wherein the mixing weight ratio of the KH-550 to the KH-792 is 1:(1.5-2).

[0025] By adopting the above technical scheme, when the silane coupling agents KH-550 and KH-792 are mixed and the mixing ratio is 1: (1.5-2), the silicone adhesive has good bonding strength with cement mortar board and metal materials, which is beneficial to improve the bonding performance between silicone adhesive and different materials, improve the versatility of silicone adhesive, and make silicone adhesive suitable for highway joints with more complex bonding environments.

[0026] Optionally, the viscosity of α,ω-dihydroxy polydimethylsiloxane is in the range of 300,000-500,000 cps, and the viscosity of the dimethyl silicone oil is in the range of 350-500 cst.

[0027] By adopting the above technical scheme, when the viscosity of α, ω-dihydroxypolydimethylsiloxane is in the range of 300000-500000cps, and the viscosity of dimethyl silicone oil is in the range of 350-500cst, the colloid not only has good extrusion properties, but also has good bonding elasticity, which is beneficial to improving the elastic recovery rate of the colloid.

[0028] Optionally, the reinforcing filler is hydrophobic nano-calcium carbonate.

[0029] By adopting the above technical solution, using hydrophobic nano calcium carbonate as a reinforcing filler is beneficial to improving the tensile strength and elongation at break of the rubber, while the hydrophobic treatment is beneficial to improving the compatibility between the reinforcing filler and the rubber, so that the reinforcing filler can be fully mixed with the rubber.

[0030] Optionally, the catalyst is dibutyltin dilaurate.

[0031] By adopting the above technical solution, dibutyltin dilaurate is used as an organic tin catalyst, which has a faster reaction efficiency and is beneficial to catalyze the hydrolysis reaction of the deketoxime type cross-linking agent, thereby significantly improving the overall curing speed of the silicone glue.

[0032] In the second aspect, the present application provides a method for preparing a super-soft road and bridge engineering joint potting silica gel, which adopts the following technical scheme:

[0033] A method for preparing super-soft road and bridge engineering joint potting silica gel comprises the following steps:

[0034] S1. After α, ω-dihydroxy polydimethylsiloxane and dimethyl silicone oil are mixed and stirred evenly, reinforcing fillers are slowly added, and stirring and dispersing are continued for 1-2 hours to obtain a base rubber material;

[0035] S2, heating the basic rubber obtained in step S1 for a period of time under vacuum, then introducing dry inert gas to balance the vacuum and cooling to room temperature, then adding a deketoxime type crosslinking agent and a silane coupling agent, maintaining a vacuum state and stirring evenly to obtain a mixed rubber;

[0036] S3, after the mixed rubber material obtained in step S2 is cooled to room temperature, dry inert gas is introduced to balance the vacuum, a catalyst and a softener are added, the vacuum state is maintained and the mixture is stirred evenly to obtain the target rubber material;

[0037] S4. Finally, dry inert gas is introduced to balance the vacuum, and the target rubber material prepared in step S3 is extruded and sealed for storage in a dry environment.

[0038] By adopting the above technical scheme, the base rubber material, the deketoxime crosslinking agent, the silane coupling agent, the catalyst, the reinforcing filler and the softener are added in steps and stirred, which can prevent the catalyst from catalyzing the deketoxime crosslinking agent to undergo a hydrolysis reaction during stirring, so that each auxiliary agent can be fully stirred and evenly mixed. Moreover, extrusion and sealing are carried out in a dry environment to prevent the deketoxime crosslinking agent from undergoing a hydrolysis reaction during long-term storage, which is conducive to extending the storage time of the silicone rubber. Secondly, the production process adopted is simple, with low energy consumption, which is conducive to mass production.

[0039] In summary, the technical solution of this application has at least one of the following beneficial effects:

[0040] 1. By adding any one of the softeners selected from fatty alcohol polyoxyethylene ether, polyethylene glycol oleate or polypropylene glycol oleate, it is helpful to improve the elongation at break and elastic recovery rate of silicone adhesive, so that silicone adhesive has good mechanical properties, and can still have good elastic deformation ability and elastic recovery ability after a long time, which is helpful to prevent the occurrence of adhesive failure caused by long-term vibration of the road.

[0041] 2. By using methyl tributylidene silane in combination with PPG-600DO, the silicone adhesive not only has a more stable overall curing speed, but also can maintain relatively excellent elongation at break and elastic recovery rate, and its comprehensive performance is relatively excellent.

[0042] 3. By mixing two silane coupling agents, KH-550 and KH-792, it is helpful to improve the interfacial bonding performance between silicone adhesive and a variety of different substrates, and to improve the bonding strength between silicone adhesive and cement mortar board, metal materials, etc., so that silicone adhesive can be used in highway joints with more complex bonding environments. DETAILED DESCRIPTION

[0043] The present application is further described in detail below with reference to embodiments and comparative examples.

[0044] The dimethyl silicone oil was purchased from Dow Corning, USA, and the viscosity was 350cs and 500cs.

[0045] The hydrophobic nano calcium carbonate was purchased from Shanghai Yuanjiang Chemical Co., Ltd., and the brand name was 303 nano activated calcium carbonate, wherein the average particle size of the nano calcium carbonate of this brand was 10-100 nm, and the surface was activated. Example

[0046] [Example 1]

[0047] A super-soft road and bridge engineering joint potting silica gel, comprising the following raw materials:

[0048] 50kg α, ω-dihydroxy polydimethylsiloxane, 30kg dimethyl silicone oil, 30kg reinforcing filler, 5kg deketoxime type cross-linking agent, 1.2kg silane coupling agent, 0.04kg catalyst, 0.8kg softener.

[0049] Among them, the viscosity of α, ω-dihydroxypolydimethylsiloxane is 400000cps, the viscosity of dimethyl silicone oil is 350cs, the reinforcing filler is hydrophobic nano-calcium carbonate, the deketoxime type cross-linking agent is methyl trisbutyl ketoxime silane, the silane coupling agent is KH-550, and the catalyst is dibutyltin dilaurate.

[0050] The softener is fatty alcohol polyoxyethylene ether, and specifically, the softener is purchased from AEO-6 of Haian Petrochemical Plant.

[0051] A method for preparing super-soft road and bridge engineering joint potting silica gel comprises the following steps:

[0052] S1. After α, ω-dihydroxy polydimethylsiloxane and dimethyl silicone oil are mixed and stirred evenly, reinforcing filler is slowly added, and stirring and dispersing are continued for 1 hour to obtain a base rubber material;

[0053] S2, raising the temperature of the basic rubber obtained in step S1 to 130° C., and maintaining the vacuum degree at -0.1 MPa for dehydration for 30 min, then introducing dry nitrogen to balance the vacuum and cooling to room temperature, then adding a deketoxime type crosslinking agent and a silane coupling agent, maintaining the vacuum degree at -0.1 MPa and stirring for 30 min to obtain a mixed rubber;

[0054] S3, after the mixed rubber material obtained in step S2 is cooled to room temperature, dry nitrogen is introduced to balance the vacuum, a catalyst and a softener are added, the vacuum degree is maintained at a vacuum state of -0.1 MPa and stirred for 30 minutes to obtain the target rubber material;

[0055] S4. Finally, dry nitrogen is introduced again to balance the vacuum, and the target rubber material prepared in step S3 is extruded and sealed in a dry environment to obtain an ultra-soft road and bridge engineering joint potting silica gel.

[0056] [Example 2]

[0057] A super-soft road and bridge engineering joint potting silica gel, comprising the following raw materials:

[0058] 60kg α, ω-dihydroxy polydimethylsiloxane, 25kg dimethyl silicone oil, 10kg reinforcing filler, 4kg deketoxime type cross-linking agent, 1kg silane coupling agent, 0.05kg catalyst, 1kg softener.

[0059] Among them, the viscosity of α, ω-dihydroxy polydimethylsiloxane is 300000cps, the viscosity of dimethyl silicone oil is 500cs, the reinforcing filler is hydrophobic nano-calcium carbonate, the deketoxime type cross-linking agent is vinyl trisbutyl ketoxime silane, the silane coupling agent is KH-792, and the catalyst is dibutyltin dilaurate.

[0060] Among them, the softener is fatty alcohol polyoxyethylene ether. Specifically, the softener is AEO-5 and AEO-10 ​​purchased from Haian Petrochemical Plant, and the mixing weight ratio of AEO-5 to AEO-10 ​​is 1:0.2, that is, the addition amount of AEO-5 is 0.833 kg, and the addition amount of AEO-10 ​​is 0.167 kg.

[0061] A method for preparing super-soft road and bridge engineering joint potting silica gel comprises the following steps:

[0062] S1. After α, ω-dihydroxy polydimethylsiloxane and dimethyl silicone oil are mixed and stirred evenly, reinforcing filler is slowly added, and stirring and dispersing are continued for 1 hour to obtain a base rubber material;

[0063] S2, raising the temperature of the base rubber obtained in step S1 to 130° C., and maintaining the vacuum degree at -0.1 MPa for dehydration for 20 min, then introducing dry nitrogen to balance the vacuum and cooling to room temperature, then adding a deketoxime type crosslinking agent and a silane coupling agent, maintaining the vacuum degree at -0.1 MPa and stirring for 30 min to obtain a mixed rubber;

[0064] S3, after the mixed rubber material obtained in step S2 is cooled to room temperature, dry nitrogen is introduced to balance the vacuum, a catalyst and a softener are added, the vacuum degree is maintained at a vacuum state of -0.1 MPa and stirred for 30 minutes to obtain the target rubber material;

[0065] S4. Finally, dry nitrogen is introduced again to balance the vacuum, and the target rubber material prepared in step S3 is extruded and sealed in a dry environment to obtain an ultra-soft road and bridge engineering joint potting silica gel.

[0066] [Example 3]

[0067] A super-soft road and bridge engineering joint potting silica gel, comprising the following raw materials:

[0068] 45kg α, ω-dihydroxy polydimethylsiloxane, 45kg dimethyl silicone oil, 40kg reinforcing filler, 8kg deketoxime type cross-linking agent, 1.5kg silane coupling agent, 0.03kg catalyst, 0.3kg softener.

[0069] The viscosity of α, ω-dihydroxy polydimethylsiloxane is 500000 cps, the viscosity of dimethyl silicone oil is 350 cs, the reinforcing filler is hydrophobic nano-calcium carbonate, the deketoxime crosslinking agent is methyl trisbutyl ketoxime silane, and the catalyst is dibutyl tin dilaurate.

[0070] The silane coupling agent is a mixture of two silane coupling agents, KH-550 and KH-792. The specific weight ratio of KH-550 to KH-792 is 1:2, that is, the addition amount of KH-550 is 0.5 kg, and the addition amount of KH-792 is 1 kg.

[0071] The softener is polyethylene glycol oleate, and specifically, the softener is PPG-400MO purchased from Haian Petrochemical Plant.

[0072] A method for preparing super-soft road and bridge engineering joint potting silica gel comprises the following steps:

[0073] S1. After α, ω-dihydroxy polydimethylsiloxane and dimethyl silicone oil are mixed and stirred evenly, reinforcing filler is slowly added, and stirring and dispersing are continued for 1 hour to obtain a base rubber material;

[0074] S2, raising the temperature of the base rubber obtained in step S1 to 130° C., and maintaining the vacuum degree at -0.1 MPa for dehydration for 20 min, then introducing dry nitrogen to balance the vacuum and cooling to room temperature, then adding a deketoxime type crosslinking agent and a silane coupling agent, maintaining the vacuum degree at -0.1 MPa and stirring for 30 min to obtain a mixed rubber;

[0075] S3, after the mixed rubber material obtained in step S2 is cooled to room temperature, dry nitrogen is introduced to balance the vacuum, a catalyst and a softener are added, the vacuum degree is maintained at a vacuum state of -0.1 MPa and stirred for 30 minutes to obtain the target rubber material;

[0076] S4. Finally, dry nitrogen is introduced again to balance the vacuum, and the target rubber material prepared in step S3 is extruded and sealed in a dry environment to obtain an ultra-soft road and bridge engineering joint potting silica gel.

[0077] [Example 4]

[0078] A super-soft silicone sealant for road and bridge engineering joints, which differs from [Example 1] in that the softener is different.

[0079] In this embodiment, the softener is fatty alcohol polyoxyethylene ether, and specifically, the softener is purchased from AEO-9 of Haian Petrochemical Plant.

[0080] [Example 5]

[0081] A super-soft silicone sealant for road and bridge engineering joints, which differs from [Example 1] in that the softener is different.

[0082] In this embodiment, the softener is fatty alcohol polyoxyethylene ether. Specifically, the softener is AEO-6 and AEO-9 purchased from Haian Petrochemical Plant, and the mixing weight ratio of AEO-6 to AEO-9 is 1:0.3, that is, the addition amount of AEO-6 is 0.615 kg, and the addition amount of AEO-9 is 0.185 kg.

[0083] [Example 6]

[0084] A super-soft silicone sealant for road and bridge engineering joints, which differs from [Example 1] in that the softener is different.

[0085] In this embodiment, the softener is polyethylene glycol oleate. Specifically, the softener is polyethylene glycol monooleate purchased from Haian Petrochemical Plant, with a brand name of PEG-400MO.

[0086] [Example 7]

[0087] A super-soft silicone sealant for road and bridge engineering joints, which differs from [Example 1] in that the softener is different.

[0088] In this embodiment, the softener is polyethylene glycol oleate. Specifically, the softener is polyethylene glycol monooleate purchased from Haian Petrochemical Plant, with a brand name of PEG-600MO.

[0089] [Example 8]

[0090] A super-soft silicone sealant for road and bridge engineering joints, which differs from [Example 1] in that the softener is different.

[0091] In this embodiment, the softener is polyethylene glycol oleate. Specifically, the softener is polyethylene glycol monooleate purchased from Haian Petrochemical Plant, with a brand name of PEG-600DO.

[0092] [Example 9]

[0093] A super-soft silicone sealant for road and bridge engineering joints, which differs from [Example 1] in that the softener is different.

[0094] In this embodiment, the softener is polyethylene glycol oleate. Specifically, the softener is polyethylene glycol monooleate purchased from Haian Petrochemical Plant, with a brand name of PPG-600DO.

[0095] [Example 10]

[0096] A super-soft road and bridge engineering joint sealing silica gel, which differs from [Example 9] in that the deketoxime type cross-linking agent is different.

[0097] In this embodiment, the deketoxime type cross-linking agent is vinyltributylacetonatoximosilane.

[0098] [Example 11]

[0099] A super-soft silicone sealant for road and bridge engineering joints, which differs from [Example 9] in the use of a different silane coupling agent.

[0100] In this embodiment, the silane coupling agent is replaced by KH792 in equal amounts.

[0101] [Example 12]

[0102] A super-soft silicone sealant for road and bridge engineering joints, which differs from [Example 9] in the use of a different silane coupling agent.

[0103] In this embodiment, the silane coupling agent is replaced by a mixture of KH-550 and KH-792 in equal amounts, and the mixing weight ratio of KH-550 to KH-792 is 1:2, that is, the addition amount of KH-550 is 0.4 kg, and the addition amount of KH-792 is 0.8 kg.

[0104] [Comparative Example 1]

[0105] A silicone adhesive, which differs from [Example 1] in that no softener is added.

[0106] [Comparative Example 2]

[0107] A kind of silicone glue, an alcohol-type silicone glue purchased from a Thai glue company on the market, the specific model is 793.

[0108] 1. Tensile bonding performance: refer to "GB / T 13477.8 Test methods for building sealing materials Part 8: Determination of tensile bonding performance" for testing, and record the tensile strength (MPa) of each embodiment and comparative example. The specific test substrates are cement mortar board and aluminum plate.

[0109] 2. Elastic recovery performance: Test according to Method A in GB / T 13477.17 Test methods for building sealing materials Part 17: Determination of elastic recovery rate, and record the elastic recovery rate of each embodiment and comparative example. If the colloid breaks during the stretching process, it will not be recorded. The specific test substrate is a cement mortar board with an initial width of 12 mm and an elongation percentage of 60%.

[0110] 3. Elastic durability: First, prepare samples according to "GB / T 13477.17 Test methods for building sealing materials Part 17: Determination of elastic recovery rate", and then perform automatic cycle exposure test aging on the prepared samples according to the provisions of Table 3 Method A Cycle No. 1 in "GB / T 16422.2-2014 Plastic Laboratory Light Source Exposure Test Method", with an exposure time of 500 h and a relative humidity of 50%. After aging, the elastic recovery performance of each embodiment and comparative example is measured again, and the elastic recovery rate (%) after aging is recorded.

[0111] 4. Curing speed: Refer to GB / T 32369-2005 Determination of the degree of curing of sealants for testing. Method 2 wedge groove method is used for testing. The test is carried out in a low temperature environment. The test temperature of the low temperature environment is -5±2℃, the ambient humidity is 60%, and the thickness (mm) of the cured silicone glue is recorded after 8h, 16h and 24h.

[0112] Table 1 Silicone rubber tensile properties test data

[0113]

[0114] Table 2 Silicone adhesive curing speed data

[0115]

[0116] Combining Example 1 with Comparative Examples 1-2 and the data in Tables 1 and 2, it can be seen that after adding a softener, the elastic recovery rate of the silicone glue can be effectively improved, and the elasticity after curing can also be close to that of the alcohol-type silicone glue, and the curing speed of the silicone glue is also slightly improved. This may be because the softener added is a fatty alcohol polyoxyethylene ether, which has a lipophilic long-chain aliphatic segment and a hygroscopic EO segment. The long-chain aliphatic segment can fully entangle with the colloid when the silicone glue is cured, thereby improving the cohesive force of the colloid itself, which is beneficial to improving the elasticity of the silicone glue after curing; and the EO segment can give the silicone glue a certain hygroscopicity. When the silicone glue is exposed to the air, the silicone glue can fully absorb moisture in the air, promote the rapid hydrolysis and reaction of the deketoxime type cross-linking agent, thereby improving the overall curing speed of the silicone glue.

[0117] Combining Example 1 with Comparative Examples 4-5 and the data in Tables 1 and 2, it can be seen that as the HLB value of the added fatty alcohol polyoxyethylene ether increases, the hydrophilicity of the softener becomes stronger, and thus its hygroscopicity is improved to a certain extent, and the initial curing speed of the silicone adhesive is significantly accelerated. However, the surface curing is too fast, and the deep layer cannot fully absorb moisture, which may cause the subsequent deep layer curing speed to slow down. Secondly, as the hydrophilicity increases, its lipophilicity is relatively weakened, which may cause the softener to be unevenly dispersed in the silicone adhesive, thereby causing a certain impact on the overall elastic recovery. When the softener AEO-6 and AEO-9 are mixed with each other in a weight ratio of 1:0.3, the silicone adhesive can show better comprehensive performance, with good elasticity and a relatively balanced and fast curing speed.

[0118] In combination with Example 1 and Example 6 and in combination with the data in Table 1 and Table 2, it can be seen that when the softener is selected from polyethylene glycol oleate, specifically when PEG-400MO is selected, compared with the selection of AEO-6, the silicone adhesive has better elasticity on the surface after curing, and also has excellent elastic recovery rate and elastic persistence, while the silicone adhesive is more uniform in overall curing speed, and can still maintain a faster speed for curing when cured to the deep layer. This may be because polyethylene glycol monooleate also has a hygroscopic EO segment and a lipophilic long-chain aliphatic segment, and the role played is roughly close to that of fatty alcohol polyoxyethylene ether, but the oleic acid segment in PEG-400MO has a high carbon content and a long oily segment, which may cause further entanglement in the silicone adhesive system and improve the mechanical properties of the silicone adhesive after curing. Secondly, the oleic acid segment contains double bonds, which may cause chain scission during the colloid curing process and react in the system, promoting the curing of silicone adhesive to a certain extent.

[0119] Combining Examples 6-8 and the data in Tables 1 and 2, it can be seen that as the molecular weight in polyethylene glycol oleate increases, the EO chain segment grows, and the hygroscopicity of the softener is improved to a certain extent, which is beneficial to improving the overall curing speed of the silicone adhesive. When the softener is polyethylene glycol dioleate, specifically PEG-600DO, the elastic recovery rate of the silicone adhesive is improved to a certain extent compared with PEG-600MO using monooleate, which indicates that the elasticity of the silicone adhesive is improved to a certain extent. This may be because the compatibility of dioleate with silicone adhesive is better than that of monooleate, and the chain segment is longer, which is conducive to the full entanglement and connection between the silicone rubbers.

[0120] Combined with the data in Examples 8-9 and Tables 1 and 2, it can be seen that when the deep curing accelerator is selected as polypropylene glycol dioleate, specifically PPG-600DO, compared with the selection of PEG-600DO, the overall curing speed of the silicone adhesive can be further improved, but the interfacial bonding strength of the silicone adhesive with other media has a small decrease. This may be because the PPG-600DO segment also includes a hygroscopic PO segment and a lipophilic long-chain aliphatic chain end, and the role played is roughly similar to that of polyethylene glycol dioleate. In addition, the compatibility of polypropylene glycol dioleate in the silicone adhesive system is better than that of polyethylene glycol dioleate. PPG-600DO can be further fully mixed in the silicone adhesive and give full play to the role of promoting the curing of the silicone adhesive. However, since the hydrophilicity of polypropylene glycol dioleate is lower than that of polyethylene glycol dioleate, the surface connectivity with most media is poor, which may affect the interfacial bonding strength of the silicone adhesive.

[0121] Combining Examples 9-10 and the data in Tables 1 and 2, it can be seen that when the softener is PPG-600DO, compared with the use of vinyl tributylacetoximate silane, the use of methyl tributylacetoximate silane as the deketoxime crosslinking agent, the overall curing speed of the silicone adhesive is more stable, and a relatively excellent elastic recovery rate can be maintained. This may be because the vinyl group in the vinyl tributylacetoximate silane will further react and increase the bonding cohesion in the colloid during the curing process, so that the curing degree and hardness of the colloid are improved, which will greatly reduce the toughness of the colloid.

[0122] Combining Example 9 and Examples 11-12 and the data in Table 1 and Table 2, it can be seen that when the silane coupling agent is KH-550, the silicone adhesive has good interfacial bonding with the aluminum plate and high bonding strength, but the bonding with the cement mortar board is low; when the silane coupling agent is KH-792, the bonding strength between the silicone adhesive and the cement mortar board can be improved, but the bonding with the aluminum plate will also be reduced accordingly; when the silane coupling agent is KH-550 and KH-792, and the mixing ratio is 1:2, the silicone adhesive has good bonding strength with metal substrates such as cement mortar boards and aluminum plates, which is conducive to the application of silicone adhesive in the potting of highway joints.

[0123] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A super soft silicone sealant for road and bridge engineering joints, characterized in that: It includes the following raw materials in parts by weight: α,ω-dihydroxy polydimethylsiloxane: 45-60 parts; Dimethyl silicone oil: 25-40 parts; Reinforcing filler: 10-40 parts; Deketoxime type cross-linking agent: 4-7 parts; Silane coupling agent: 0.8-1.6 parts; Catalyst: 0.03-0.05 parts; Softener: 0.3-1 part; Among them, the viscosity range of the α, ω-dihydroxy polydimethylsiloxane is 300000-500000cps, the viscosity range of the dimethyl silicone oil is 350-500cst; the reinforcing filler is hydrophobic nano-calcium carbonate; the deketoxime type crosslinking agent is methyl tributylidene oxime silane, and the softener is PPG-600DO.

2. The super soft road and bridge engineering joint potting silica gel according to claim 1 is characterized by: The silane coupling agent is a mixture of two silane coupling agents, KH-550 and KH-792, wherein the mixing weight ratio of the KH-550 to the KH-792 is 1:(1.5-2).

3. The super soft road and bridge engineering joint potting silica gel according to claim 1 is characterized by: The catalyst is dibutyltin dilaurate.

4. A method for preparing super-soft road and bridge engineering joint potting silica gel, characterized in that: The method for preparing the super-soft road and bridge engineering joint sealing silica gel according to any one of claims 1 to 3 comprises the following steps: S1. After α, ω-dihydroxy polydimethylsiloxane and dimethyl silicone oil are mixed and stirred evenly, reinforcing fillers are slowly added, and stirring and dispersing are continued for 1-2 hours to obtain a base rubber material; S2, heating the basic rubber obtained in step S1 for a period of time under vacuum, then introducing dry inert gas to balance the vacuum and cooling to room temperature, then adding a deketoxime type crosslinking agent and a silane coupling agent, maintaining a vacuum state and stirring evenly to obtain a mixed rubber; S3, after the mixed rubber material obtained in step S2 is cooled to room temperature, dry inert gas is introduced to balance the vacuum, a catalyst and a softener are added, the vacuum state is maintained and the mixture is stirred evenly to obtain the target rubber material; S4. Finally, dry inert gas is introduced to balance the vacuum, and the target rubber material obtained in step S3 is extruded and sealed for storage in a dry environment.