A highly stable light metal hydride and its preparation method
By alternately depositing metal oxide and organic polymer nanofilms on the surface of light metal hydrides, the stability problem of light metal hydrides is solved, and efficient improvement of water, oxygen and thermal stability is achieved, making it suitable for solid propellants and high-energy explosives.
Patent Information
- Application Number
- CN202410124934.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-30
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-01-30
AI Technical Summary
Light metal hydrides suffer from poor chemical and thermal stability in hydrogen storage materials, especially AlH3 and MgH2, which have poor water and oxygen sensitivity and compatibility, affecting their application in solid propellants.
Atomic layer deposition (ALD) and molecular layer deposition (MLD) techniques are used to alternately deposit metal oxide nanofilms and organic polymer nanofilms on the surface of light metal hydrides, forming a dense composite film layer that improves the water and oxygen stability and thermal stability of the material.
Precise and controllable coating of nanofilms on the surface of light metal hydrides has been achieved, significantly improving the water and oxygen stability and thermal stability of the materials, making them suitable for solid propellants and high-energy explosives.
Smart Images

Figure CN118255641B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of light metal hydride technology, and relates to the surface modification of light metal hydrides, specifically to a highly stable light metal hydride and its preparation method. Background Technology
[0002] Light metal hydrides, represented by AlH3 and MgH2, are typical solid-state hydrogen storage materials. Due to their high hydrogen content, high calorific value, and low relative molecular mass of combustion products, they are considered ideal hydrogen energy carriers for improving the energy performance of solid propellants, attracting widespread attention both domestically and internationally. Replacing some aluminum powder in the propellant formulation with light metal hydrides can reduce the average molecular mass of the combustion gases in the combustion chamber, increase the isobaric and isochoric specific heat capacities of the combustion products, and improve the propellant's characteristic velocity and specific impulse.
[0003] Although light metal hydrides show promising application prospects in solid propellant systems, these materials still face some insurmountable bottlenecks in their application, severely restricting their scope and progress. For example, AlH3 possesses advantages such as high hydrogen storage capacity (volume hydrogen storage of 0.148 kg / L, more than twice the density of liquid hydrogen; mass hydrogen storage reaches 10.08%), fast hydrogen release rate (rapid hydrogen release at temperatures below 100℃), high calorific value (theoretical calorific value of aluminum powder is 1.3 times), and non-toxicity, making it considered the most promising solid propellant fuel. However, as a metastable solid, AlH3 exhibits poor chemical and thermal stability, spontaneously decomposing during storage. Furthermore, AlH3 has poor compatibility with nitrate ester components in propellants, leading to increased system sensitivity and hazard when added to solid propellants, thus affecting its application. For example, MgH2 has a hydrogen storage capacity of 7.6% by mass and an enthalpy change of 74.5 kJ / mol for hydrogen release. It also exhibits high chemical and thermal stability (hydrogen release temperature around 300°C). Theoretical studies have shown that using MgH2 as an additive in solid propellants and explosives can significantly improve their energy levels and explosive power. However, MgH2 has poor air stability, is sensitive to water and oxygen, and has poor compatibility with commonly used propellant components, which limits its widespread application.
[0004] All of the above relate to the core issue of the surface properties of light metal hydrides. Modifying the surface chemical composition and structure of light metal hydrides is a primary means of improving material stability and safety. Surface modification techniques can be used to modify the surface and interface of light metal hydrides, forming a complete, dense, and controllable thickness inert modification layer on the material surface. This alters the surface state of the material, isolates the active species from direct contact with the environment, and enhances material stability.
[0005] Chinese invention patent number ZL 202010721214.3 discloses an α-AlH3 / Al2O3 / C 60 A double-shell structured complex, its synthesis method, and its applications. This method involves acid pickling and passivation followed by an organic liquid-phase method to form alumina and C on the surface of α-AlH3, respectively. 60 Double-shell structures are used to improve the stability of α-AlH3. Chinese invention patent ZL202010699289.6 discloses a method for improving the thermal stability of α-AlH3. This method uses acid washing and polymer coating to form an alumina and a polycarbazole double-shell structure on the surface of α-AlH3, respectively, to improve its stability. Chinese invention patents ZL 202011073333.9 and ZL202011073319.9 disclose an α-AlH3-EVOH double-shell structure composite, its preparation method and application, and an α-AlH3-PVDF double-shell structure composite, its preparation method and application, respectively. These methods all involve first passivating α-AlH3 by acid washing, then oxidizing the surface to form an alumina film, and finally coating the passivated α-AlH3 surface with a polymer layer, thereby improving the stability of α-AlH3 through the double-shell structure.
[0006] The disadvantages of the methods disclosed above are that the coating process is completed in an organic liquid phase, the process is complex, and the product needs to be separated by means of filtration and solvent evaporation, requiring a large amount of manual operation. In addition, these methods lack precise control over the coating process, the coating layer thickness is difficult to adjust precisely, and the integrity, uniformity, and density of the coating layer are poor, which can easily lead to the loss of hydrogen content in the metal hydride. Summary of the Invention
[0007] In view of the shortcomings of the existing technology, the purpose of this invention is to provide a highly stable light metal hydride and its preparation method, thereby solving the technical problem that the water and oxygen stability and thermal stability of light metal hydrides in the prior art need to be further improved.
[0008] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:
[0009] A highly stable light metal hydride, wherein the highly stable light metal hydride has a light metal hydride core, and odd-numbered shells and even-numbered shells are alternately arranged on the surface of the core from the inside to the outside.
[0010] The light metal hydrides are lithium hydride (LiH), aluminum hydride (AlH3), magnesium hydride (MgH2), or zirconium hydride (ZrH2).
[0011] The odd-numbered shells are metal oxide nanofilms.
[0012] The even-numbered shells are organic polymer nanofilms.
[0013] The metal oxide nanofilm is deposited on the surface of a light metal hydride using atomic layer deposition technology.
[0014] The organic polymer nanofilm is deposited on the surface of a metal oxide nanofilm using molecular layer deposition technology.
[0015] The present invention also has the following technical features:
[0016] Preferably, the metal oxide nanofilm is an aluminum oxide film, a magnesium oxide film, a zirconium oxide film, or a silicon oxide film.
[0017] Preferably, the organic polymer nanofilm is a polyurea film, a polyamide film, a polyimide film, a polyurethane film, a polyethylene terephthalate film, or a polythiourea film.
[0018] Specifically, the sum of the masses of the metal oxide nanofilm and the organic polymer nanofilm accounts for 0.1% to 5% of the total mass of the highly stable light metal hydride.
[0019] Preferably, the sum of the masses of the metal oxide nanofilm and the organic polymer nanofilm accounts for 4.8% of the total mass of the highly stable light metal hydride.
[0020] Specifically, the total thickness of the metal oxide nanofilm and the organic polymer nanofilm is 0.1–200 nm.
[0021] Preferably, the total thickness of the metal oxide nanofilm and the organic polymer nanofilm is 20 nm.
[0022] Preferably, the particle size of the light metal hydride is in the range of micrometers to nanometers.
[0023] This invention also protects a method for preparing a highly stable light metal hydride as described above, characterized in that the method is carried out according to the following steps:
[0024] Step S1: The light metal hydride is loaded into the reactor, and then the reactor is loaded into the reaction chamber of the atomic layer deposition system or the molecular layer deposition system. The lid of the reaction chamber is closed, and a vacuum is drawn to control the pressure in the reaction chamber at 1 to 1000 Pa. At the same time, the reaction chamber is heated to keep the temperature of the reaction chamber at 30°C to 300°C and the temperature of the precursor at room temperature to 200°C.
[0025] Step S2: Initiate an atomic layer deposition reaction on the surface of a light metal hydride using an atomic layer deposition system. One atomic layer deposition reaction includes the following sub-steps:
[0026] Step S201: The first reaction precursor is injected into the reaction chamber to undergo a saturated chemisorption reaction with the surface groups of the light metal hydride for a time of t1.
[0027] Step S202: Inert carrier gas is introduced to remove excess first reaction precursor and reaction byproducts for time t2.
[0028] Step S203: The second type of reaction precursor is injected into the reaction chamber to undergo a surface exchange reaction with the first type of precursor groups adsorbed on the surface of the light metal hydride for a time of t3.
[0029] Step S204: Inert carrier gas is introduced to remove excess second reaction precursor and reaction byproducts for time t4.
[0030] Step S3 involves repeating the atomic layer deposition reaction m times, i.e., repeating step S2, to form a light metal hydride with a light metal hydride core and a nano-metal oxide film as the first coating layer.
[0031] Step S4: Molecular layer deposition reaction is initiated on the surface of the light metal hydride modified by the first coating layer using a molecular layer deposition system. One molecular layer deposition reaction includes the following sub-steps:
[0032] Step S401: Inject the third type of reaction precursor into the reaction chamber to undergo a saturated chemisorption reaction with the surface groups of the modified light metal hydride for a time of t5.
[0033] Step S401: Inert carrier gas is introduced to remove excess third reaction precursor and reaction byproducts for time t6.
[0034] Step S403: The fourth type of reaction precursor is injected into the reaction chamber to undergo a surface exchange reaction with the third type of precursor groups adsorbed on the surface of the modified light metal hydride for a time of t7.
[0035] Step S404: Inert carrier gas is introduced to remove excess fourth reaction precursor and reaction byproducts for time t8.
[0036] Step S5 involves repeating the molecular layer deposition reaction n times, i.e., repeating step S4, to form a modified light metal hydride with a light metal hydride core, a nano-metal oxide film as the first modification layer, and a polymer nano-film as the second modification layer.
[0037] Step S6: Following the alternating order of step S3 followed by step S5, step S3 and step S5 are repeated p times to form a highly stable light metal hydride.
[0038] Preferably, in step S1, the temperature of the reaction chamber is between 70°C and 160°C, and the temperature of the precursor is between 30°C and 150°C.
[0039] Preferably, the first reaction precursor includes trimethylaluminum, triethylaluminum, magnesium thiocene, ethyl magnesium thiocene, tetra(dimethylamino)zirconium, tetra(methylethylamino)zirconium, silicon tetrachloride, tetra(dimethylamino)silicon, or tetra(methylethylamino)silicon.
[0040] Preferably, the second reaction precursor includes water, hydrogen peroxide, oxygen, or ozone.
[0041] Preferably, the third reaction precursor includes adipic acid chloride, terephthaloyl chloride, pyromellitic dianhydride, terephthalaldehyde, terephthalic diisocyanate, or 1,4-butanediisocyanate.
[0042] Preferably, the fourth reaction precursor is ethylenediamine, 1,6-hexanediamine, p-phenylenediamine, 4,4'-diaminodiphenyl ether, 4-aminophenol, ethylene glycolamine, ethylene glycol, glycerol, or 1,4-phenylenediol.
[0043] Preferably, the inert carrier gas is nitrogen, helium, or argon.
[0044] Preferably, t1, t3, t5 and t7 are 1 to 2000 s; t2, t4, t6 and t8 are 5 to 4000 s.
[0045] More preferably, t1, t3, t5 and t7 are 5 to 100 s; t2, t4, t6 and t8 are 10 to 150 s.
[0046] Preferably, the number of cycles m and n are 1 to 2000 times, and p is 1 to 1000.
[0047] More preferably, the number of cycles m and n are 15 to 160 times, and p is 1 to 3.
[0048] Compared with the prior art, the present invention has the following technical effects:
[0049] (I) The metal oxide and polymer nanofilms of the present invention can be uniformly and completely coated on the surface of light metal hydride according to a pre-designed structure. The composition and content of the surface nanofilm can be precisely controlled by adjusting the number of atomic and molecular layer deposition cycles.
[0050] (II) Based on the synergistic effect of dense metal oxide film and hydrophobic polymer film, the water and oxygen stability and thermal stability of light metal hydrides modified by composite film coating are significantly improved.
[0051] (III) The preparation method adopted in this invention belongs to the gas-solid interface reaction. The light metal hydride is in the solid phase, and the surface nanofilm is deposited on the solid phase surface through the reaction of gas molecules. After the reaction is completed, the light metal hydride can be used directly without post-processing. Moreover, the method has a high degree of automation, good repeatability of the preparation process, and can realize the surface treatment of samples in the range of grams to kilograms. It is easy to promote and apply in industry.
[0052] (IV) This invention employs atomic layer deposition to deposit light metal hydrides into metal oxide-polymer nanocomposite films, resulting in significantly improved surface hydrophobicity, water-oxygen stability, and thermal stability. The light metal hydrides prepared by this invention can be applied in fields such as solid propellants and high-energy explosives. Attached Figure Description
[0053] Figure 1 XPS spectra of the original AlH3 sample, AlH3@Al2O3@PU-(80 / 160)*1 sample, and AlH3@Al2O3@PU-(40 / 80)*2 sample in Examples 1-2.
[0054] Figure 2 The images show the contact angles of the original AlH3 sample and the AlH3@Al2O3@PU-(80 / 160)*1 sample in Example 1.
[0055] Figure 3 The images show TEM images of the original AlH3 sample and the AlH3@Al2O3@PU-(80 / 160)*1 sample from Example 1.
[0056] Figure 4 The thermal stability test diagrams are shown for the original AlH3 sample and the AlH3@Al2O3@PU-(80 / 160)*1 sample in Example 1.
[0057] Figure 5 The graphs show the water-oxygen stability test results of the original AlH3 sample and the AlH3@Al2O3@PU-(80 / 160)*1 sample in Example 1.
[0058] Figure 6 The images show the contact angles of the original AlH3 sample and the AlH3@Al2O3@PU-(40 / 80)*2 sample in Example 2.
[0059] Figure 7 TEM images of the original AlH3 sample and the AlH3@Al2O3@PU-(40 / 80)*2 sample from Example 2.
[0060] Figure 8The thermal stability test diagrams are shown for the original AlH3 sample and the AlH3@Al2O3@PU-(40 / 80)*2 sample in Example 2.
[0061] Figure 9 The graphs show the water-oxygen stability test results of the original AlH3 sample and the AlH3@Al2O3@PU-(40 / 80)*2 sample in Example 2.
[0062] Figure 10 SEM images of the original MgH2 sample and the MgH2@ZrO2@PI-(15 / 30)*3 sample from Example 3.
[0063] Figure 11 The graphs show the water-oxygen stability test results of the original MgH2 sample and the MgH2@ZrO2@PI-(15 / 30)*3 sample in Example 3.
[0064] The specific content of the present invention will be further explained in detail below with reference to the embodiments. Detailed Implementation
[0065] It should be noted that, unless otherwise specified, all materials and devices used in this invention are those known in the art.
[0066] In this invention, the atomic layer deposition system and the molecular layer deposition system are commonly used known atomic layer deposition systems and molecular layer deposition systems. The reactor structure of the atomic layer deposition system and the molecular layer deposition system is a fixed bed type, a rotating bed type, and a fluidized bed type. The mass of the light metal hydride charged in the reactor is 0.1 to 1000 grams.
[0067] The characterization instruments and equipment used in this invention include X-ray photoelectron spectroscopy (Thermo Scientific K-Alpha XPS), scanning electron microscope (FEIQuanta 600FEG SEM), field emission transmission electron microscope (FEITecnai G2 F20S-TWIN), contact angle tester, constant temperature test chamber, and PCT curve tester.
[0068] In this invention, the average particle size of aluminum hydride and magnesium hydride used is divided into the hundreds of micrometers and the tens of micrometers.
[0069] In this invention, the number-average molecular weight of the polymers selected for the organic polymer nanofilm will vary with the number of deposition cycles in the molecular layer deposition process, with the preferred number-average molecular weight being in the range of 200 to 400.
[0070] The number average molecular weight of polyurea is 2,000 to 180,000, with a preferred value of 80,000.
[0071] The number average molecular weight of the polyamide is 2,000 to 90,000, with a preferred value of 45,000.
[0072] The number average molecular weight of polyimide is 2800 to 120000, with a preferred value of 60000.
[0073] The number average molecular weight of polyurethane is 2200 to 220000, with a preferred value of 85000.
[0074] The number average molecular weight of polyethylene terephthalate is 2,000 to 100,000, with a preferred value of 40,000.
[0075] The number average molecular weight of polythiourea is 2,500 to 200,000, with a preferred value of 100,000.
[0076] The following are specific embodiments of the present invention. It should be noted that the present invention is not limited to the following specific embodiments. All equivalent modifications made based on the technical solutions of this application fall within the protection scope of the present invention.
[0077] Example 1:
[0078] This embodiment provides a highly stable light metal hydride and its preparation method, which is carried out according to the following steps:
[0079] Step S1: 0.5 g of AlH3 is loaded into a fixed-bed reactor, and then the reactor is loaded into the reaction chambers of the atomic layer deposition system and the molecular layer deposition system. The lid of the reaction chamber is closed, and a vacuum is drawn to control the pressure in the reaction chamber at 50 Pa. At the same time, the reaction chamber is heated to a temperature of 70 °C. The precursors trimethylaluminum and water are at room temperature, terephthalic acid diisocyanate is at 50 °C, and ethylenediamine is at 30 °C.
[0080] Step S2: Initiate the atomic layer deposition reaction on the AlH3 surface. One atomic layer deposition reaction includes the following sub-steps:
[0081] Step S201: The first reaction precursor, trimethylaluminum, is injected into the reaction chamber to undergo a saturated chemisorption reaction with the surface groups of AlH3 for 5 seconds.
[0082] Step S202: Inert carrier gas nitrogen is introduced to remove excess first reaction precursor and reaction byproducts for 10 seconds.
[0083] Step S203: The second type of reaction precursor water is injected into the reaction chamber to undergo a surface exchange reaction with the first type of precursor groups adsorbed on the AlH3 surface for 5 seconds.
[0084] Step S204: Inert carrier gas nitrogen is introduced to remove excess second reaction precursor and reaction byproducts for 15 seconds.
[0085] Step S3 involves 80 cycles of atomic layer deposition, which is equivalent to repeating step S2 80 times to form a modified AlH3@Al2O3 sample with AlH3 as the core and a nano-Al2O3 thin film as the first coating layer.
[0086] Step S4: Molecular layer deposition reaction begins on the surface of the modified AlH3@Al2O3 sample. One molecular layer deposition reaction includes the following sub-steps:
[0087] Step S401: The third reaction precursor, terephthalic diisocyanate, is injected into the reaction chamber to undergo a saturated chemisorption reaction with the surface groups of the modified AlH3@Al2O3 sample for 8 seconds.
[0088] Step S402: Inert carrier gas nitrogen is introduced to remove excess third reaction precursor and reaction byproducts for 15 seconds.
[0089] In step S403, the fourth reaction precursor, ethylenediamine, is injected into the reaction chamber to undergo a surface exchange reaction with the third precursor groups adsorbed on the surface of the modified AlH3@Al2O3 sample for 10 seconds.
[0090] Step S404: Inert carrier gas nitrogen is introduced to remove excess fourth reaction precursor and reaction byproducts for 20 seconds.
[0091] Step S5 involves 160 cycles of molecular layer deposition reaction, i.e., repeating step S4 160 times, to form an AlH3@Al2O3@PU modified AlH3 sample with AlH3 as the core, a nano-Al2O3 film as the first modification layer, and a polymer nanofilm PU as the second modification layer.
[0092] Step S6: Following the order of step S3 followed by step S5, step S3 and step S5 are repeated once to form modified AlH3 with AlH3 as the core, a nano-Al2O3 thin film as the first modification layer, and a polymer nano-thin film as the second modification layer, wherein the mass ratio of the coating film is 4.8%.
[0093] Figure 1 XPS test results show that after 80 cycles of Al2O3 and 160 cycles of polyurea nanofilm coating, the Al signal on the AlH3 surface is significantly weakened, the N signal is significantly enhanced, and the impurity Cl signal disappears, indicating that the polyurea nanofilm with a thickness of only about 20 nm has achieved complete and uniform coating of the aluminum hydride sample.
[0094] Figure 2The contact angle test results show that the surface hydrophobicity of the AlH3 sample modified by composite film coating is significantly improved, with the contact angle jumping from 32° to 121°.
[0095] Figure 3 TEM results showed that the thickness of the composite nanofilm coated on the AlH3 surface was about 20 nm. There was obvious interfacial delamination between the alumina nanofilm and the polyurea film (two layers, with the alumina nanofilm as the first layer and the polyurea nanofilm as the second layer). The coating film was completely, uniformly and densely covering the AlH3 surface.
[0096] Figure 4 The thermal stability characterization experiment was carried out under vacuum conditions at 100℃. As shown in the figure, within the same time period, the hydrogen release pressure of the AlH3 sample coated with composite nanofilm was significantly lower than that of the original sample, indicating that the thermal stability of the sample modified by composite nanofilm coating was significantly higher than that of the original aluminum hydride sample.
[0097] Figure 5 The results of the damp heat stability test showed that under extreme temperature and humidity conditions of 35℃ and 95% humidity, compared with the uncoated AlH3 original sample, the AlH3 sample coated with composite nanofilm had a moisture absorption weight gain rate of only 2.23% after 15 days of storage, which was much smaller than the 11.1% of the original sample. This further illustrates the excellent water and oxygen barrier properties of the composite nanofilm.
[0098] Example 2:
[0099] This embodiment provides a highly stable light metal hydride and its preparation method, which is carried out according to the following steps:
[0100] Step S1: 200g of AlH3 is loaded into a rotating bed reactor, and then the reactor is loaded into the reaction chambers of the atomic layer deposition system and the molecular layer deposition system. The lid of the reaction chamber is closed, and a vacuum is drawn to control the pressure in the reaction chamber at 200Pa. At the same time, the reaction chamber is heated to a temperature of 70°C, while the precursors trimethylaluminum and water are at room temperature, terephthalic acid diisocyanate is at 50°C, and ethylenediamine is at 30°C.
[0101] Step S2: Initiate the atomic layer deposition reaction on the AlH3 surface. One atomic layer deposition reaction includes the following sub-steps:
[0102] Step S201: The first reaction precursor, trimethylaluminum, is injected into the reaction chamber to undergo a saturated chemisorption reaction with the surface groups of AlH3 for 100 s.
[0103] Step S202: Inert carrier gas nitrogen is introduced to remove excess first reaction precursor and reaction byproducts for 150 s.
[0104] Step S203: The second type of reaction precursor water is injected into the reaction chamber to undergo a surface exchange reaction with the first type of precursor groups adsorbed on the AlH3 surface for 100 seconds.
[0105] Step S204: Inert carrier gas nitrogen is introduced to remove excess second reaction precursor and reaction byproducts for 180 s.
[0106] Step S3 involves 40 cycles of atomic layer deposition, which is equivalent to repeating step S2 40 times to form a modified AlH3@Al2O3 sample with AlH3 as the core and a nano-Al2O3 thin film as the first coating layer.
[0107] Step S4: Molecular layer deposition reaction begins on the surface of the modified AlH3@Al2O3 sample. One molecular layer deposition reaction includes the following sub-steps:
[0108] Step S401: The third reaction precursor, terephthalic diisocyanate, is injected into the reaction chamber to undergo a saturated chemisorption reaction with the surface groups of the modified AlH3@Al2O3 sample for 100 s.
[0109] Step S402: Inert carrier gas nitrogen is introduced to remove excess third reaction precursor and reaction byproducts for 120 seconds.
[0110] In step S403, the fourth reaction precursor, ethylenediamine, is injected into the reaction chamber to undergo a surface exchange reaction with the third precursor groups adsorbed on the surface of the modified AlH3@Al2O3 sample for 80 seconds.
[0111] Step S404: Inert carrier gas nitrogen is introduced to remove excess fourth reaction precursor and reaction byproducts for 100 s.
[0112] Step S5 involves 80 cycles of molecular layer deposition reaction, i.e., repeating step S4 80 times, to form an AlH3@Al2O3@PU modified AlH3 sample with AlH3 as the core, a nano-Al2O3 film as the first modification layer, and a polymer nanofilm PU as the second modification layer.
[0113] Step S6: Following the order of step S3 followed by step S5, step S3 and step S5 are repeated twice to form modified AlH3 with AlH3 as the core, nano-Al2O3 thin film as the first and third modification layers, and polymer nano-film PU as the second and fourth modification layers.
[0114] Figure 6 The contact angle test results show that the surface hydrophobicity of the AlH3 sample modified by composite film coating is significantly improved, with the contact angle jumping from 32° to 114°.
[0115] Figure 7 TEM results showed that the thickness of the composite nanofilm coated on the AlH3 surface was about 20 nm. There was obvious interfacial delamination between the alumina nanofilm and the polyurea film (4 layers, with the alumina nanofilm as the first and third layers and the polyurea film as the second and fourth layers). The coating film was completely, uniformly and densely covering the AlH3 surface.
[0116] Figure 8 The thermal stability characterization experiment was carried out under vacuum conditions at 100℃. As shown in the figure, within the same time period, the hydrogen release pressure of the AlH3 sample coated with composite nanofilm was significantly lower than that of the original sample, indicating that the thermal stability of the sample modified by composite nanofilm coating was significantly higher than that of the original aluminum hydride sample.
[0117] Figure 9 The results of the damp heat stability test showed that under extreme temperature and humidity conditions of 35℃ and 95% humidity, compared with the uncoated AlH3 original sample, the AlH3 sample coated with composite nanofilm had a moisture absorption weight gain rate of only 2.66% after 15 days of storage, which was much smaller than the 11.1% of the original sample. This further illustrates the excellent water and oxygen barrier properties of the composite nanofilm.
[0118] Example 3:
[0119] This embodiment provides a highly stable light metal hydride and its preparation method, which is carried out according to the following steps:
[0120] Step S1: 10 grams of MgH2 is loaded into a fluidized bed reactor, and then the reactor is loaded into the reaction chambers of the atomic layer deposition system and the molecular layer deposition system. The lid of the reaction chamber is closed, and a vacuum is drawn to control the pressure in the reaction chamber at 133 Pa. At the same time, the reaction chamber is heated to a temperature of 160°C, the precursor tetra(dimethylamino)zirconium is at 80°C, pyromellitic dianhydride is at 150°C, and ethylenediamine and water are at 25°C.
[0121] Step S2, the atomic layer deposition reaction begins on the MgH2 surface. One atomic layer deposition reaction includes the following sub-steps:
[0122] Step S201: The first reaction precursor, tetra(dimethylamino)zirconium, is injected into the reaction chamber to undergo a saturated chemisorption reaction with the surface groups of MgH2 for 30 seconds.
[0123] Step S202: Inert carrier gas nitrogen is introduced to remove excess first reaction precursor and reaction byproducts for 40 seconds.
[0124] Step S203: The second type of reaction precursor water is injected into the reaction chamber to undergo a surface exchange reaction with the first type of precursor groups adsorbed on the MgH2 surface for 25 seconds.
[0125] Step S204: Inert carrier gas nitrogen is introduced to remove excess second reaction precursor and reaction byproducts for 50 seconds.
[0126] Step S3 involves 15 cycles of atomic layer deposition, which is equivalent to repeating step S2 15 times to form a modified MgH2@ZrO2 sample with MgH2 as the core and a nano ZrO2 thin film as the first coating layer.
[0127] Step S4: Molecular layer deposition reaction begins on the surface of the modified MgH2@ZrO2 sample. One molecular layer deposition reaction includes the following sub-steps:
[0128] Step S401: The third reaction precursor, pyromellitic dianhydride, is injected into the reaction chamber to undergo a saturated chemisorption reaction with the surface groups of the modified MgH2@ZrO2 sample for 30 seconds.
[0129] Step S402: Inert carrier gas nitrogen is introduced to remove excess third reaction precursor and reaction byproducts for 45 seconds.
[0130] In step S403, the fourth reaction precursor, ethylenediamine, is injected into the reaction chamber to undergo a surface exchange reaction with the third precursor groups adsorbed on the surface of the modified MgH2@ZrO2 sample for 30 seconds.
[0131] Step S404: Inert carrier gas nitrogen is introduced to remove excess fourth reaction precursor and reaction byproducts for 30 seconds.
[0132] Step S5 involves 30 cycles of molecular layer deposition reaction, i.e., repeating step S4 30 times, to form a MgH2@ZrO2@PI modified MgH2 sample with MgH2 as the core, nano ZrO2 film as the first modification layer, and polymer nanofilm PI as the second modification layer.
[0133] Step S6: Following the order of step S3 followed by step S5, step S3 and step S5 are repeated three times in sequence to form modified MgH2 with MgH2 as the core, nano ZrO2 thin film as the first, third and fifth modification layers, and polymer nanofilm PI as the second, fourth and sixth modification layers.
[0134] Figure 10SEM results showed that the morphology of magnesium hydride particles coated with the zirconium oxide and polyimide composite nanofilm remained intact and was basically consistent with that of untreated magnesium hydride particles. This indicates that the composite nanofilm can grow uniformly on the surface of magnesium hydride samples, and the nanoscale coating layer does not change the original morphology of the magnesium hydride particles.
[0135] Figure 11 The results of the damp heat stability test showed that, under the temperature and humidity conditions of 30℃ and 80% humidity, compared with the uncoated original magnesium hydride sample, the magnesium hydride sample coated with composite nanofilm had a moisture absorption weight gain rate of only 3.1% after 8 days of storage, which was much smaller than the 58% of the original sample. This further illustrates the excellent water and oxygen barrier properties of the composite nanofilm.
Claims
1. A method for preparing a highly stable light metal hydride, characterized in that, This method is performed according to the following steps: Step S1: 0.5 g of AlH3 is loaded into a fixed-bed reactor, and then the reactor is loaded into the reaction chamber of the atomic layer deposition system and the molecular layer deposition system. The lid of the reaction chamber is closed, and a vacuum is drawn to control the pressure in the reaction chamber at 50 Pa. At the same time, the reaction chamber is heated to a temperature of 70 °C. The precursors trimethylaluminum and water are at room temperature, terephthalic diisocyanate is at 50 °C, and ethylenediamine is at 30 °C. Step S2: Initiate the atomic layer deposition reaction on the AlH3 surface. One atomic layer deposition reaction includes the following sub-steps: Step S201: The first reaction precursor, trimethylaluminum, is injected into the reaction chamber to undergo a saturated chemisorption reaction with the surface groups of AlH3 for 5 seconds. Step S202: Inert carrier gas nitrogen is introduced to remove excess first reaction precursor and reaction byproduct for 10 seconds. Step S203: The second type of reaction precursor water is injected into the reaction chamber to undergo a surface exchange reaction with the first type of precursor groups adsorbed on the AlH3 surface for 5 seconds. Step S204: Inert carrier gas nitrogen is introduced to remove excess second reaction precursor and reaction byproducts for 15 seconds. Step S3 involves 80 cycles of atomic layer deposition, which is equivalent to repeating step S2 80 times to form a modified AlH3@Al2O3 sample with AlH3 as the core and a nano-Al2O3 thin film as the first coating layer. Step S4: Molecular layer deposition reaction begins on the surface of the modified AlH3@Al2O3 sample. One molecular layer deposition reaction includes the following sub-steps: Step S401: The third reaction precursor, terephthalic diisocyanate, is injected into the reaction chamber to undergo a saturated chemical adsorption reaction with the surface groups of the modified AlH3@Al2O3 sample for 8 seconds. Step S402: Inert carrier gas nitrogen is introduced to remove excess third reaction precursor and reaction byproducts for 15 seconds. Step S403: The fourth reaction precursor, ethylenediamine, is injected into the reaction chamber to undergo a surface exchange reaction with the third precursor groups adsorbed on the surface of the modified AlH3@Al2O3 sample for 10 seconds. Step S404: Inert carrier gas nitrogen is introduced to remove excess fourth reaction precursor and reaction byproducts for 20 seconds. Step S5 involves 160 cycles of molecular layer deposition reaction, i.e., repeating step S4 160 times to form an AlH3@Al2O3@PU modified AlH3 sample with AlH3 as the core, a nano-Al2O3 film as the first modification layer, and a polymer nanofilm PU as the second modification layer; the PU is polyurethane. Step S6: Following the order of step S3 followed by step S5, step S3 and step S5 are repeated once to form modified AlH3 with AlH3 as the core, a nano-Al2O3 thin film as the first modification layer, and a polymer nano-thin film as the second modification layer.
2. A method for preparing a highly stable light metal hydride, characterized in that, This method is performed according to the following steps: Step S1: 200g of AlH3 is loaded into a rotating bed reactor, and then the reactor is loaded into the reaction chamber of the atomic layer deposition system and the molecular layer deposition system. The lid of the reaction chamber is closed, and a vacuum is drawn to control the pressure in the reaction chamber at 200Pa. At the same time, the reaction chamber is heated to a temperature of 70°C, the precursor trimethylaluminum and water are at room temperature, terephthalic diisocyanate is at 50°C, and ethylenediamine is at 30°C. Step S2: Initiate the atomic layer deposition reaction on the AlH3 surface. One atomic layer deposition reaction includes the following sub-steps: Step S201: The first reaction precursor, trimethylaluminum, is injected into the reaction chamber to undergo a saturated chemisorption reaction with the surface groups of AlH3 for 100 s. Step S202: Inert carrier gas nitrogen is introduced to remove excess first reaction precursor and reaction byproducts for 150 s. Step S203: The second type of reaction precursor water is injected into the reaction chamber to undergo a surface exchange reaction with the first type of precursor groups adsorbed on the AlH3 surface for 100 seconds. Step S204: Inert carrier gas nitrogen is introduced to remove excess second reaction precursor and reaction byproducts for 180 s. Step S3 involves 40 cycles of atomic layer deposition, which is equivalent to repeating step S2 40 times to form a modified AlH3@Al2O3 sample with AlH3 as the core and a nano-Al2O3 thin film as the first coating layer. Step S4: Molecular layer deposition reaction begins on the surface of the modified AlH3@Al2O3 sample. One molecular layer deposition reaction includes the following sub-steps: Step S401: The third reaction precursor, terephthalic diisocyanate, is injected into the reaction chamber to undergo a saturated chemical adsorption reaction with the surface groups of the modified AlH3@Al2O3 sample for 100 s. Step S402: Inert carrier gas nitrogen is introduced to remove excess third reaction precursor and reaction byproducts for 120 seconds. Step S403: The fourth reaction precursor, ethylenediamine, is injected into the reaction chamber to undergo a surface exchange reaction with the third precursor groups adsorbed on the surface of the modified AlH3@Al2O3 sample for 80 seconds. Step S404: Inert carrier gas nitrogen is introduced to remove excess fourth reaction precursor and reaction byproducts for 100 seconds. Step S5 involves 80 cycles of molecular layer deposition reaction, i.e., repeating step S4 80 times to form an AlH3@Al2O3@PU modified AlH3 sample with AlH3 as the core, a nano-Al2O3 film as the first modification layer, and a polymer nanofilm PU as the second modification layer; the PU is polyurethane. Step S6: Following the order of step S3 followed by step S5, step S3 and step S5 are repeated twice to form modified AlH3 with AlH3 as the core, nano-Al2O3 thin film as the first and third modification layers, and polymer nano-film PU as the second and fourth modification layers.
3. A method for preparing a highly stable light metal hydride, characterized in that, This method is performed according to the following steps: Step S1: 10 grams of MgH2 is loaded into a fluidized bed reactor, and then the reactor is loaded into the reaction chamber of the atomic layer deposition system and the molecular layer deposition system. The lid of the reaction chamber is closed, and a vacuum is drawn to control the pressure in the reaction chamber at 133 Pa. At the same time, the reaction chamber is heated to a temperature of 160°C, the precursor tetra(dimethylamino)zirconium is at 80°C, the pyromellitic dianhydride is at 150°C, and the ethylenediamine and water are at 25°C. Step S2, the atomic layer deposition reaction begins on the MgH2 surface. One atomic layer deposition reaction includes the following sub-steps: Step S201: The first reaction precursor tetra(dimethylamino)zirconium is injected into the reaction chamber to undergo a saturated chemisorption reaction with the surface groups of MgH2 for 30 seconds. Step S202: Inert carrier gas nitrogen is introduced to remove excess first reaction precursor and reaction byproducts for 40 seconds. Step S203: The second type of reaction precursor water is injected into the reaction chamber to undergo a surface exchange reaction with the first type of precursor groups adsorbed on the MgH2 surface for 25 seconds. Step S204: Inert carrier gas nitrogen is introduced to remove excess second reaction precursor and reaction byproducts for 50 seconds. Step S3 involves 15 cycles of atomic layer deposition, which is equivalent to repeating step S2 15 times to form a modified MgH2@ZrO2 sample with MgH2 as the core and a nano ZrO2 thin film as the first coating layer. Step S4: Molecular layer deposition reaction begins on the surface of the modified MgH2@ZrO2 sample. One molecular layer deposition reaction includes the following sub-steps: Step S401: The third reaction precursor, pyromellitic dianhydride, is injected into the reaction chamber to undergo a saturated chemical adsorption reaction with the surface groups of the modified MgH2@ZrO2 sample for 30 seconds. Step S402: Inert carrier gas nitrogen is introduced to remove excess third reaction precursor and reaction byproducts for 45 seconds. Step S403: The fourth reaction precursor, ethylenediamine, is injected into the reaction chamber to undergo a surface exchange reaction with the third precursor groups adsorbed on the surface of the modified MgH2@ZrO2 sample for 30 seconds. Step S404: Inert carrier gas nitrogen is introduced to remove excess fourth reaction precursor and reaction byproducts for 30 seconds. Step S5 involves 30 cycles of molecular layer deposition reaction, i.e., repeating step S4 30 times to form a MgH2@ZrO2@PI modified MgH2 sample with MgH2 as the core, a nano ZrO2 film as the first modification layer, and a polymer nanofilm PI as the second modification layer; wherein PI is polyimide. Step S6: Following the order of step S3 followed by step S5, step S3 and step S5 are repeated three times in sequence to form modified MgH2 with MgH2 as the core, nano ZrO2 thin film as the first, third and fifth modification layers, and polymer nanofilm PI as the second, fourth and sixth modification layers.
Citation Information
Patent Citations
Alpha-AlH3 / Al2O3 / C60 double-shell structure compound as well as synthesis method and application thereof
CN111892468A
Method for improving thermal stability of alpha-AlH3
CN111908991A
An α-AlH3-PVDF double-shell composite, its preparation method and application
CN112266313B
An α-AlH3-EVOH double-shell complex, its preparation method and application
CN112279742B
Aluminum hydride surface coating modification method
CN104046957A