UV resin ink with excellent water resistance and preparation method thereof

Through specific formulation and sonication technology, the problem of poor water resistance of UV resin inks is solved, and the ink is high water resistance and stability is achieved, ensuring that the printed materials maintain a good appearance and quality in various environments.

CN118256111BActive Publication Date: 2024-11-08YINGDE AOMARKANG POLYMER NEW MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410440362.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-12
Publication Date
2024-11-08
Estimated Expiration
2044-04-12

Smart Images

  • Figure BDA0004788950310000091
    Figure BDA0004788950310000091
  • Figure BDA0004788950310000101
    Figure BDA0004788950310000101
Patent Text Reader

Abstract

The present application relates to the field of ink technology, and specifically discloses a UV resin ink with excellent water resistance and a preparation method thereof. A UV resin ink with excellent water resistance includes 50-80 parts of UV resin; 15-20 parts of 2-benzoylbenzoic acid glycidyl ester; 10-20 parts of β-alanine ethanol solution; 8-30 parts of pigment; 1-5 parts of dispersant; 2-8 parts of fluorocarbon solvent. The UV resin ink with excellent water resistance of the present application can be used in the field of ink printing. The ink formula contains a variety of selected ingredients, and each ingredient is reasonably configured in terms of weight fraction. This precise ratio helps to ensure the stable performance and reliable quality of the ink. The ink has excellent water resistance, can maintain good stability in various environments, and is not easy to fade, smudge or fall off.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of inks, and more specifically, to an ink containing UV resins with excellent water resistance and a preparation method thereof. Background Art

[0002] UV resin ink is an ink that uses ultraviolet light curing technology. It has the characteristics of fast curing, high gloss and color stability, good adhesion, wear resistance, scratch resistance, chemical stability, suitability for a variety of substrates and environmental protection. It can be quickly dried and cured under ultraviolet light, improve production efficiency, make the appearance quality of printed products excellent, and can also be firmly attached to various substrates. It has good durability and resistance to a variety of chemical substances. It can also be used for a variety of substrates such as paper, plastic, metal, etc., and may contain less volatile organic compounds (VOCs) than traditional inks.

[0003] In the related art, for example, the application document with application number CN202311727945.9 discloses a flexible UV ink and a preparation method thereof, wherein the flexible UV ink comprises the following raw materials by weight: 40-85 parts of resin, 10-40 parts of active monomer, 2-8 parts of photoinitiator and 1-10 parts of filler, wherein the resin comprises one or more of acrylic resin, acrylic resin containing flexible segments or polyurethane modified acrylic resin. The flexible UV ink provided by the present invention is intended to improve the flexibility and adhesion of the UV ink.

[0004] However, the inks in the above-mentioned technologies have the problem of poor water resistance. When in contact with water, the inks may fade or discolor, thus affecting the appearance and quality of the printed products. Summary of the invention

[0005] In order to improve the water resistance of ink and thus ensure the appearance and quality of printed products, the present application provides a UV resin-containing ink with excellent water resistance and a preparation method thereof.

[0006] In the first aspect, the present application provides a UV resin ink with excellent water resistance using the following technical solution:

[0007] A UV resin ink with excellent water resistance, comprising the following raw materials in weight fractions:

[0008] 50-80 parts of UV resin;

[0009] 2-benzoylbenzoic acid glycidyl ester 15-20 parts;

[0010] 10-20 parts of β-alanine ethanol solution;

[0011] Pigment 8-30 parts;

[0012] Dispersant 1-5 parts;

[0013] 2-8 parts of fluorocarbon solvents

[0014] By adopting the above technical scheme, a small amount of 2-benzoylbenzoic acid glycidyl ester is used as a photoinitiator to quickly initiate the photocuring reaction, thereby reducing the amount of photoinitiator used, avoiding the phenomenon that the polymer product becomes hydrophilic after being placed for a long time due to excessive amount of photoinitiator during polymerization, and thus improving the water resistance of the ink. The β-alanine ethanol solution helps to improve the solubility and compatibility of the ink, further enhancing the water resistance, stability and printing effect of the ink. The ink formula contains a variety of selected ingredients, and each ingredient is reasonably configured in terms of weight fraction. This precise ratio helps to ensure the stable performance and reliable quality of the ink. The ink has excellent water resistance, can maintain good stability in various environments, and is not easy to fade, smudge or fall off.

[0015] Optionally, the UV resin is isobornyl epoxy acrylate.

[0016] By adopting the above technical solution and using isobornyl epoxy acrylate, this type of resin has good chemical stability and durability, thus providing the ink with better weather resistance and chemical corrosion resistance, and extending the service life of the ink.

[0017] Optionally, the pigment is a color powder, and the pigment is any one of iron oxide powder and titanium dioxide.

[0018] By adopting the above technical solution, the pigment is limited to either iron oxide or titanium dioxide, both of which have excellent color performance and stability, ensuring that the color of the ink is bright and lasting, and is not easily affected by external factors and discolored.

[0019] Optionally, the mass concentration of the β-alanine ethanol solution is 15-20%.

[0020] By adopting the above technical solution, the β-alanine ethanol solution helps to improve the solubility and compatibility of the ink, and further enhances the water resistance, stability and printing effect of the ink. The β-alanine ethanol solution within the above concentration range has the most significant enhancement effect on the water resistance of the ink.

[0021] Optionally, the dispersant includes any one of water glass, sodium tripolyphosphate and polyethylene glycol.

[0022] By adopting the above technical solution, the above dispersant can effectively disperse the pigment particles in the ink system, prevent the pigment from agglomerating, and keep the pigment in a good dispersed state. It can also enhance the stability of the ink, avoid precipitation, stratification and other problems, and reduce the amount of pigment used, thereby reducing printing costs.

[0023] Optionally, the fluorocarbon solvent is ethyl perfluoroacetate.

[0024] By adopting the above technical solution, ethyl perfluoroacetate is selected as the fluorocarbon solvent, which has good solubility and volatility, and helps the ink to maintain good water resistance.

[0025] In a second aspect, the present application provides a method for preparing a UV resin ink having excellent water resistance, using the following technical solution:

[0026] A method for preparing a UV resin ink with excellent water resistance comprises the following steps:

[0027] S1. Accurately weigh the components by weight: UV resin, 2-benzoylbenzoic acid glycidyl ester, β-alanine ethanol solution, pigment, dispersant and fluorocarbon solvent;

[0028] S2. Add the pigment to the dispersant and stir evenly to ensure that the pigment is fully dispersed;

[0029] S3, adding UV resin, 2-benzoylbenzoic acid glycidyl ester, and β-alanine ethanol solution to the above pigment dispersion, and continuing to stir and mix;

[0030] S4. Slowly add fluorocarbon solvent while continuously stirring to fully blend all components;

[0031] S5. During the stirring process, ultrasonic treatment is performed and stirring is performed for 3-10 minutes to form a uniform ink.

[0032] By adopting the above technical scheme, the preparation method has the characteristics of relatively simple operation and wide applicability by accurately weighing each component, stirring and mixing in steps and controlling the addition speed, performing ultrasonic treatment and controlling the stirring time. It can ensure the accurate composition of the ink, sufficient dispersion of the pigment, and sufficient fusion of the components, so that stable, uniform, high-quality and excellent water-resistant ink can be quickly obtained.

[0033] In summary, this application has the following beneficial effects:

[0034] 1. The ink of this application uses a small amount of 2-benzoylbenzoic acid glycidyl ester as a photoinitiator to reduce the amount of photoinitiator, avoid hydrophilicity, and improve water resistance. At the same time, the addition of β-alanine ethanol solution further enhances the water resistance, stability and printing effect of the ink.

[0035] 2. The ink of this application uses acrylic UV resin, which has good chemical stability and durability, provides better weather resistance and chemical corrosion resistance, and extends the service life of the ink.

[0036] 3. The ink of the present application uses dispersants such as water glass, sodium tripolyphosphate or polyethylene glycol to effectively disperse the pigment particles, prevent pigment agglomeration, maintain a good dispersion state, enhance ink stability, reduce precipitation and stratification problems, and reduce printing costs.

[0037] 4. The method of the present application first accurately weighs each component by weight, stirs and mixes step by step, performs ultrasonic treatment and controls the stirring time. The method is relatively simple to operate and has wide applicability, ensuring that the ink composition is accurate, the pigment is fully dispersed, and the components are fully integrated, so as to quickly obtain high-quality ink with excellent water resistance. DETAILED DESCRIPTION

[0038] The present application is further described in detail below with reference to the embodiments.

[0039] Various raw materials used in the examples and preparation examples of the present application are commercially available, among which:

[0040] Acrylic UV resin was purchased from Wuhan Hyperbranched Resin Technology Co., Ltd.; 2-benzoylbenzoic acid glycidyl ester was purchased from Shanghai Jizhi Biochemical Technology Co., Ltd., with a purity of 98.0%; β-alanine was purchased from Shandong Siyang Biotechnology Co., Ltd., with an effective substance content of 99.0%; ethyl perfluoroacetate was purchased from Hubei Mackays Fine Chemical Technology Co., Ltd., with a purity of 99.0%.

[0041] Example

[0042] Example 1

[0043] A UV resin ink with excellent water resistance, the raw material components and applications of which are shown in Table 1, wherein the pigment is iron oxide powder; the dispersant is water glass; the fluorocarbon solvent is perfluoroethyl acetate; the mass concentration of the β-alanine ethanol solution is 15%.

[0044] A UV resin ink with excellent water resistance is prepared by the following method:

[0045] S1. Accurately weigh the components by weight: isobornyl epoxyacrylate, 2-benzoylbenzoic acid glycidyl ester, β-alanine ethanol solution, iron oxide powder, water glass and ethyl perfluoroacetate;

[0046] S2. Add iron oxide powder into water glass and stir evenly to ensure that the iron oxide powder is fully dispersed;

[0047] S3, adding isobornyl epoxyacrylate, 2-benzoylbenzoic acid glycidyl ester, and β-alanine ethanol solution to the above pigment dispersion, and continuing to stir and mix;

[0048] S4, slowly add ethyl perfluoroacetate while continuously stirring to allow all components to fully blend;

[0049] S5. During the stirring process, ultrasonic treatment is performed and stirring is performed for 3 minutes to form a uniform ink.

[0050] Example 2

[0051] A UV resin ink with excellent water resistance, the raw material components and applications of which are shown in Table 1, wherein the pigment is iron oxide powder; the dispersant is water glass; the fluorocarbon solvent is perfluoroethyl acetate; the mass concentration of the β-alanine ethanol solution is 15%.

[0052] A UV resin ink with excellent water resistance is prepared by the following method:

[0053] S1. Accurately weigh the components by weight: isobornyl epoxyacrylate, 2-benzoylbenzoic acid glycidyl ester, β-alanine ethanol solution, iron oxide powder, water glass and ethyl perfluoroacetate;

[0054] S2. Add iron oxide powder into water glass and stir evenly to ensure that the iron oxide powder is fully dispersed;

[0055] S3, adding isobornyl epoxyacrylate, 2-benzoylbenzoic acid glycidyl ester, and β-alanine ethanol solution to the above pigment dispersion, and continuing to stir and mix;

[0056] S4, slowly add ethyl perfluoroacetate while continuously stirring to allow all components to fully blend;

[0057] S5. During the stirring process, ultrasonic treatment is performed and stirring is performed for 7 minutes to form a uniform ink.

[0058] Example 3

[0059] A UV resin ink with excellent water resistance, the raw material components and applications of which are shown in Table 1, wherein the pigment is iron oxide powder; the dispersant is water glass; the fluorocarbon solvent is perfluoroethyl acetate; the mass concentration of the β-alanine ethanol solution is 15%.

[0060] A UV resin ink with excellent water resistance is prepared by the following method:

[0061] S1. Accurately weigh the components by weight: isobornyl epoxyacrylate, 2-benzoylbenzoic acid glycidyl ester, β-alanine ethanol solution, iron oxide powder, water glass and ethyl perfluoroacetate;

[0062] S2. Add iron oxide powder into water glass and stir evenly to ensure that the iron oxide powder is fully dispersed;

[0063] S3, adding isobornyl epoxyacrylate, 2-benzoylbenzoic acid glycidyl ester, and β-alanine ethanol solution to the above pigment dispersion, and continuing to stir and mix;

[0064] S4, slowly add ethyl perfluoroacetate while continuously stirring to allow all components to fully blend;

[0065] S5. During the stirring process, ultrasonic treatment is performed and stirring is performed for 7 minutes to form a uniform ink.

[0066] Table 1 Raw material components and dosage in Examples 1-3 (kg)

[0067] project Example 1 Example 2 Example 3 Isobornyl Epoxyacrylate 50 65 80 2-Benzoylbenzoic acid glycidyl ester 15 18 20 β-Alanine ethanol solution 10 15 20 pigment 8 20 30 Dispersants 1 3 5 Fluorocarbon solvents 2 5 8

[0068] Example 4

[0069] A UV resin ink with excellent water resistance, which is different from Example 3 in that the mass concentration of the β-alanine ethanol solution in this example is 18%.

[0070] Example 5

[0071] A UV resin ink with excellent water resistance, which is different from Example 3 in that the mass concentration of the β-alanine ethanol solution in this example is 20%.

[0072] Example 6

[0073] A UV resin ink with excellent water resistance, which is different from Example 3 in that the mass concentration of the β-alanine ethanol solution in this example is 5%.

[0074] Example 7

[0075] A UV resin ink with excellent water resistance, which is different from Example 3 in that the mass concentration of the β-alanine ethanol solution in this example is 35%.

[0076] Example 8

[0077] A UV resin ink with excellent water resistance, which is different from Example 3 in that the dispersant in this example is sodium tripolyphosphate.

[0078] Example 9

[0079] A UV resin ink with excellent water resistance, which is different from Example 3 in that the dispersant in this example is polyethylene glycol.

[0080] Comparative Example

[0081] Comparative Example 1

[0082] A UV resin ink with excellent water resistance, which is different from Example 8 in that the UV resin in this example is propylene acetate.

[0083] Comparative Example 2

[0084] A UV resin ink with excellent water resistance, which is different from Example 8 in that the UV resin in this embodiment is propylene glycol butyl ester.

[0085] Comparative Example 3

[0086] A UV resin ink with excellent water resistance, which is different from Example 8 in that an equal amount of acetone is used instead of the β-alanine ethanol solution in this example.

[0087] Comparative Example 4

[0088] A UV resin ink with excellent water resistance, which is different from Example 8 in that an equal amount of benzophenone is used in this example instead of 2-benzoylbenzoic acid glycidyl ester.

[0089] Performance testing

[0090] The inks of Examples 1-9 and Comparative Examples 1-4 were subjected to performance tests, and the experimental results are shown in Table 2.

[0091] Among them, the water resistance test method is: put the cloth printed with PET silk screen ink into a washing machine, the temperature is 50℃, wash for 8 hours, and observe whether there is obvious shedding.

[0092] Table 2 Test results of Examples 1-9 and Comparative Examples 1-4

[0093]

[0094]

[0095] It can be seen from the test results in Table 2 that the water resistance of Examples 1-5 and 8-9 is good. After 8 hours of water washing machine test, all of them are 100% free of shedding. The water resistance of Examples 6 and 7 is slightly worse, with 2% and 3% shedding respectively. The water resistance of Comparative Examples 1-4 is obviously poorer, with a higher proportion of shedding, which are 20%, 20%, 15% and 25% respectively. The viscosity of the ink prepared by Examples 1-9 ranges from 13000cps to 16000cps. However, the viscosity of Comparative Examples 1-4 is relatively high, ranging from 18000cps to 27000cps.

[0096] It can be seen that the ink provided in Examples 1-3 of the present application has good water resistance. Since isobornyl epoxy acrylate is used as the UV resin base material, it has the advantages of fast curing speed, high hardness, good water resistance and good yellowing resistance. Therefore, the prepared ink has good water resistance. However, since propylene acetate and propylene ethyl butyrate are used as UV resin base materials in Comparative Examples 1 and 2, the prepared inks have about 20% shedding phenomenon under water washing conditions, so the water resistance is poor.

[0097] In comparative example 3, an equal amount of acetone was used to replace the β-alanine ethanol solution, and the ink finally showed 15% shedding phenomenon under the condition of water washing, indicating that the β-alanine ethanol solution has a good effect on improving the water resistance of the ink. The β-alanine ethanol solution helps to improve the solubility and compatibility of the ink, and further enhances the water resistance and stability of the ink.

[0098] In Comparative Example 4, an equal amount of benzophenone was used to replace 2-benzoylbenzoic acid glycidyl ester, and the final ink also showed 25% shedding phenomenon under the condition of water washing, indicating that the use of 2-benzoylbenzoic acid glycidyl ester as a photoinitiator has a good effect on improving the water resistance of the ink. 2-Benzoylbenzoic acid glycidyl ester has a good initiation catalytic effect on UV curing reaction. Using a small amount of 2-benzoylbenzoic acid glycidyl ester as a photoinitiator can quickly initiate the photocuring reaction, thereby reducing the amount of photoinitiator, avoiding the phenomenon that the polymerization product becomes hydrophilic after being placed for a long time due to excessive amount of photoinitiator during polymerization, thereby improving the water resistance of the ink.

[0099] From the test results in Table 2, we can get the following more detailed summary:

[0100] The inks of Examples 1-5 and 8-9 exhibited excellent water resistance, and after an 8-hour water washing machine test, there was no shedding at all. However, the water resistance of Examples 6 and 7 was slightly inferior, with a small amount of shedding. In contrast, the water resistance of Comparative Examples 1-4 was significantly poorer, with a higher proportion of shedding.

[0101] In terms of viscosity, the viscosity of the ink prepared in Examples 1-9 is between 13000 cps and 16000 cps, while the viscosity of the ink prepared in Comparative Examples 1-4 is higher, between 18000 cps and 27000 cps.

[0102] Further analysis shows that Examples 1-3 use isobornyl epoxyacrylate as the UV resin base material, which makes the ink have excellent water resistance. Comparative Examples 1 and 2 use propylene acetate and propylene ethyl butyrate as the UV resin base materials, respectively, resulting in poor water resistance of the ink. In Comparative Example 3, acetone is used instead of β-alanine ethanol solution, which also affects the water resistance of the ink. β-alanine ethanol solution helps to improve the solubility and compatibility of the ink, and enhances water resistance and stability.

[0103] In Comparative Example 4, benzophenone was used instead of 2-benzoylbenzoic acid glycidyl, which also had a negative impact on water resistance. 2-Benzoylbenzoic acid glycidyl, as a photoinitiator, has a good effect on improving the water resistance of ink. It can better initiate the photocuring reaction, reduce the amount of photoinitiator, avoid the phenomenon of hydrophilicity after long-term storage due to excessive dosage, and thus improve the water resistance of ink.

[0104] In summary, the ink of the embodiment of the present application performs well in terms of water resistance, which is due to the specific selection and proportion of ingredients. The comparative example shows poor water resistance through different substitutions or changes. This provides us with a valuable reference for further optimizing the ink formula and helps to develop ink products with better performance.

[0105] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A UV resin ink with excellent water resistance, characterized in that: The invention comprises the following raw materials in parts by weight: 50-80 parts of isobornyl epoxy acrylate; 2-benzoylbenzoic acid glycidyl ester 15-20 parts; 10-20 parts of β-alanine ethanol solution; Pigment 8-30 parts; Dispersant 1-5 parts; 2-8 parts of fluorocarbon solvent; The mass concentration of the β-alanine ethanol solution is 15-20%.

2. The UV resin ink with excellent water resistance according to claim 1, characterized in that: The pigment is color powder, and the pigment is any one of iron oxide powder and titanium dioxide.

3. The UV resin ink with excellent water resistance according to claim 1, characterized in that: The dispersant is any one of water glass, sodium tripolyphosphate and polyethylene glycol.

4. The UV resin ink with excellent water resistance according to claim 1, characterized in that: The fluorocarbon solvent is ethyl perfluoroacetate.

5. A method for preparing a UV resin ink having excellent water resistance as claimed in claim 1, characterized in that: The steps include: S1. Accurately weigh the components by weight: isobornyl epoxyacrylate, 2-benzoylbenzoic acid glycidyl ester, β-alanine ethanol solution, pigment, dispersant and fluorocarbon solvent; S2. Add the pigment to the dispersant and stir evenly to ensure that the pigment is fully dispersed; S3, adding UV resin, 2-benzoylbenzoic acid glycidyl ester, and β-alanine ethanol solution to the above pigment dispersion, and continue stirring and mixing; S4. Slowly add fluorocarbon solvent while continuously stirring to fully blend all components; S5. During the stirring process, ultrasonic treatment is performed and stirring is performed for 3-10 minutes to form a uniform ink.

Citation Information

Cited By

  • Low-temperature water-resistant ink for printing PE shrink film and preparation method of low-temperature water-resistant ink

    CN119639274A