A polyurethane antistatic super wear-resistant floor coating and its preparation method and application

Through surface-modified talc powder and single-wall carbon nanotube-mesoporous silica composite technology, the agglomeration of conductive materials and stress concentration in polyurethane floor coatings is solved, and the wear resistance and anti-static of the coating film are improved. Performance, achieving more uniform dispersion and higher durability.

CN118256133BActive Publication Date: 2024-11-19深圳市朗迈新材料科技有限公司
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410349414.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-26
Publication Date
2024-11-19
Estimated Expiration
2044-03-26

AI Technical Summary

Technical Problem

The agglomeration and adsorption of conductive materials in polyurethane floor coatings, as well as the coating film is prone to cracks and low tensile strength under stress.

Method used

By surface-modifying the talc powder and interacting with polyurethane resin, combined with single-wall carbon nanotubes and mesoporous silica, a stable silica gel composite film is formed, which enhances dispersion and reduces friction coefficient and forms a hard The mesh structure is used to improve wear resistance and anti-static properties.

Benefits of technology

It significantly improves the tensile strength and wear resistance of the coating film, improves the anti-static properties, reduces the generation of static charges, and improves the durability and impact resistance of the coating.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a polyurethane antistatic super wear-resistant floor coating and a preparation method and application thereof, and relates to the technical field of polyurethane. The invention modifies a talcum powder filler by a titanate coupling agent and then adds the talcum powder filler to a polyurethane resin to obtain component A, and then uses mesoporous silica as a carrier of single-walled carbon nanotubes to obtain an antistatic material component B with good dispersibility and not easy to agglomerate, and mixes component A, component B with wear-resistant material nano-alumina to obtain the floor coating. Compared with the prior art, the invention mainly solves the problems of easy agglomeration and adsorption of conductive materials in polyurethane floor coatings, as well as the problems of cracks and low tensile strength when the floor coating film is subjected to stress.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane, and in particular to a polyurethane antistatic super wear-resistant floor coating and a preparation method and application thereof. Background Art

[0002] The full name of polyurethane is polyurethane, which is a polymer compound with good heat resistance, cold resistance, toughness and strength, wear resistance, chemical resistance, weather resistance, sound absorption, electrical insulation and other properties. Polyurethane is widely used in the fields of construction, automobile, aviation, home appliances, etc. In the construction field, polyurethane is mainly used to produce waterproof coatings, thermal insulation materials, floor coatings, etc. In the automotive field, polyurethane is mainly used to produce car seats, body parts, sound insulation materials, etc. Polyurethane seats have good elasticity and comfort, which can improve riding comfort and safety; in the field of home appliances, it is mainly reflected in heat insulation, durability, waterproofing, sealing and other aspects. Polyurethane is the most commonly used insulation material for manufacturing refrigerators, air conditioners, ovens, water heaters and other home appliances.

[0003] Floor coatings protect the ground and play the role of dustproof, wear-resistant, clean and moisture-proof, so they are widely used in modern industrial floors, commercial floors, garage floors, etc. Polyurethane floor coatings have become an important choice for floor decoration and protection, and their application range is becoming more and more extensive, including factories, workshops, hospitals, schools, shopping malls, parking lots, airports and other places. In terms of performance, polyurethane floor coatings have excellent wear resistance, chemical resistance, weather resistance, waterproofness, anti-static and aesthetic characteristics, which can meet the use requirements of different places. At the same time, polyurethane floor coatings also have good construction performance and maintenance performance, simple construction, easy cleaning and maintenance. With people's attention to environmental protection and sustainable development, the research and application of polyurethane floor coatings will continue to advance, such as the development of more environmentally friendly raw materials, the promotion of water-based polyurethane floor coatings, etc. The development prospects of polyurethane floor coatings are still broad.

[0004] CN106398504A discloses an antistatic nano polyurethane floor paint, comprising the following components in parts by weight: 66-80 parts of waterborne polyurethane resin, 13-15 parts of diethylene glycol butyl ether acetate, 16-18 parts of polypropylene fiber, 5-8 parts of nano zinc oxide, 16-20 parts of polyvinyl alcohol emulsion, 6-8 parts of octyl glycidyl ether, 5-9 parts of nano titanium nitride, 5-9 parts of butyl acetate, 4.5-6.5 parts of nano nickel oxide, 3-5 parts of ethylene glycol dimethacrylate, 3-6 parts of alkyl betaine, 6-8 parts of vinyl trimethoxy silane, 1-4 parts of butyl titanate, and 8-11 parts of urea; it also comprises 8-10 parts of dimethyl ammonium sulfonate, 7-10 parts of toluene diisocyanate, and 6-12 parts of nano silicon carbide. The invented anti-static nano polyurethane floor paint can effectively prevent static electricity, is environmentally friendly, green, and has strong weather resistance. The paint film surface is smooth, hard, wear-resistant, pressure-resistant, impact-resistant, and has good corrosion resistance. It can provide effective protection, has a long service life, and is easy to construct.

[0005] CN112431377A discloses a special antistatic super wear-resistant thin layer material and construction method for the ground of a gas station and oil depot, which includes a primer, a leveling layer, an intermediate layer and a surface layer from bottom to top, wherein the primer is a high-permeability epoxy resin, the leveling layer is a liquid epoxy resin, the intermediate layer comprises a liquid epoxy resin and a polyurethane, and the surface layer is prepared by mixing and stirring component A and component B, wherein component A is made of modified polyurethane prepolymer and epoxy resin as raw materials, and modified carbon fiber and modified polyvinylidene fluoride are introduced in the preparation process, and the obtained floor has excellent wear resistance and is effectively antistatic. The polyurethane prepolymer and the epoxy resin are interlaced to form a mesh structure, so that the product has good wear resistance and antistatic properties. Modified polyvinylidene fluoride is obtained by modifying polyvinylidene fluoride with 3-aminopropyltrimethoxysilane and methyltrichlorosilane, enriching branching after modification, enriching microscopic mesh structure, and further improving wear resistance and antistatic properties. Spiral carbon fiber has good wear resistance and conductivity. The modified carbon fiber is made of spiral nanocarbon fiber as raw material, and vanadium and zinc doping are introduced using vanadyl sulfate and zinc stearate, which effectively avoids technical problems such as damage to anti-static performance caused by uneven mixing or cracking, and further improves the wear resistance of the product.

[0006] All of the above patents increase the conductivity between objects by adding inorganic conductive media such as silicon carbide and carbon fiber to polyurethane resin to play an anti-static role; however, the tiny inorganic particles have a large surface area and are easy to adsorb other additives, making them unable to play their role effectively, affecting their outward diffusion and dispersibility, and affecting the overall anti-static properties of the floor coating. Summary of the invention

[0007] In view of the above-mentioned defects of the prior art, the technical problems to be solved by the present invention are the agglomeration and adsorption problems of conductive materials in polyurethane floor coatings, and the problems of cracks and low tensile strength of floor coatings when subjected to stress.

[0008] To achieve the above-mentioned purpose, the present invention provides a polyurethane antistatic super wear-resistant floor coating and a preparation method and application thereof.

[0009] The preparation method of the polyurethane antistatic super wear-resistant floor coating comprises the following steps, measured in parts by weight:

[0010] (1) adding 0.1-0.5 parts of isopropyl titanate triisostearate to 0.1-1 parts of liquid paraffin and dispersing for 10-30 minutes, adding 10-15 parts of talc, stirring at 90-100° C. for 10-30 minutes, cooling to room temperature, adding to 60-80 parts of polyurethane and stirring for 0.5-1 hour, then adding 0.5-1 parts of wetting agent, 0.5-2 parts of dispersant, 0.1-0.8 parts of defoaming agent, and 10-30 parts of pigment, mixing and dispersing for 10-30 minutes, and grinding with a sand mill to a fineness of 40-50 μm to obtain component A;

[0011] (2) adding 15-20 parts of ethyl silicate to 150-180 parts of anhydrous ethanol, adding 120-150 parts of water to dilute, adjusting the pH value to acidic with hydrochloric acid, stirring at room temperature for 2-4 hours, and ultrasonically treating at 20-30w for 1-2 hours to obtain silica gel, adding 5-8 parts of single-walled carbon nanotubes, and continuing to stir for 1-2 hours to obtain single-walled carbon nanotube-gel for standby use;

[0012] (3) adding 5-15 parts of 10-30wt.% sodium hydroxide aqueous solution to 400-450 parts of water and stirring at room temperature for 10-20 minutes, adding 10-15 parts of single-walled carbon nanotube-gel, 15-20 parts of water, and 15-20 parts of 5-8wt.% hexadecyltrimethylammonium bromide aqueous solution, ultrasonically dispersing at 20-30w for 10-30 minutes, stirring at 75-85°C for 1-2 hours, adding 5-10 parts of ethyl silicate at 75-85°C, reacting at 75-85°C for 6-8 hours, cooling to room temperature and filtering, washing the filter cake with water and filtering, washing the filter cake with methanol and filtering, repeating the methanol washing and filtering operation 4-6 times, and drying at 50-60°C for 1-3 hours to obtain component B;

[0013] (4) Add 80-120 parts of component A, 10-15 parts of component B, and 10-15 parts of nano-alumina to 30-50 parts of water, stir at room temperature at a rate of 1000-1200 r / min for 0.5-1 hour, and filter to obtain a polyurethane antistatic and super wear-resistant floor coating.

[0014] The polyurethane in step (1) is an aqueous polyurethane resin, preferably 30-40 wt.% of the aqueous polyurethane resin.

[0015] The wetting agent in step (1) is an organosilicon wetting agent; preferably any one of QHL 606, TY-1699, Hydropalat WE3220, BYK-348 and BYK-333.

[0016] In the step (1), the dispersant is any one of BYK-110, BYK-190, BYK-161 and BYK-163.

[0017] The defoaming agent in step (1) is dimethyl silicone oil.

[0018] The pigment in step (1) is one or a mixture of more than one of carbon black, black iron oxide, red iron oxide, titanium white, phthalocyanine, fast yellow, and chrome yellow.

[0019] The hydrochloric acid in step (2) is 10-37 wt. % hydrochloric acid.

[0020] In the step (2), adjusting the pH value to acidic is adjusting the pH value to 2-4.

[0021] Talc powder is added as filler to polyurethane to improve the physical properties of polyurethane coating; unmodified powder cannot be effectively dispersed in the components due to its high surface activity. The surface of talc powder is modified by isopropyl triisostearate titanate. Monoalkoxy titanate coupling agent can directly couple with trace hydroxyl groups adsorbed on the surface of talc powder through alkoxy groups to produce chemical bonding on the interface, forming a monomolecular film on the surface of inorganic talc powder, while there is no multimolecular film on the interface of polyurethane resin. The excess titanate coupling agent after modification changes the surface energy, greatly reduces the viscosity, and reduces the adsorption and agglomeration of particles. The surface-modified talc enhances the interaction between talc and polyurethane matrix, and significantly inhibits the formation of stress concentration points around talc particles, and the hardness of polyurethane coating is also greatly improved; it is dispersed into smaller particles under the action of sand grinding by a grinder, and is more evenly and densely dispersed when added to polyurethane floor coatings, effectively dispersing the stress concentration generated at the cracks when the coating is subjected to stress, thereby effectively improving the tensile strength and wear resistance of the coating.

[0022] Single-walled carbon nanotubes have excellent conductivity, and at the same time have a large aspect ratio and specific surface area. Compared with carbon black particles, a small amount of single-walled carbon nanotubes can form a conductive network chain. Single-walled carbon nanotubes are white powder and do not affect the color of the pigment in the floor coating. Single-walled carbon nanotubes and mesoporous silica can play a good compounding and synergistic role. Ethyl silicate is used as a precursor and dissolved in ethanol, and then water is added to hydrolyze. Ethoxy groups are replaced by hydroxyl groups in water to obtain sol. The sol is continuously polycondensed to obtain silica gel, and then the pH value is adjusted to acidic to obtain stable silica gel; single-walled carbon nanotubes are added to the silica gel to obtain single-walled carbon nanotube gel, and then the single-walled carbon nanotube gel is added to the synthesized mesoporous silica. The mesoporous silica has a large specific surface area, orderly pores, and adjustable pore size. The polygonal adjacent three-dimensional network structure composed of silicon-oxygen bonds can be used as a carrier of the single-walled carbon nanotube to obtain an antistatic material component B with good dispersibility and not easy to agglomerate. After modification, the surface of the antistatic material particles has a layer of silica gel composite film, which further reduces the friction coefficient and thus inhibits and reduces the generation of static charge. At the same time, the silica gel wraps the antistatic material and then disperses it ultrasonically. The gel on the surface of the particles slowly polymerizes between the particles after aging, which promotes a dense three-dimensional Si-O-Si network. It is then added to organic polyurethane and solution. Compared with single single-walled carbon nanotubes or mesoporous silica particles, the stability and dispersibility are improved.

[0023] Nano-alumina has excellent wear resistance and greatly improves the wear resistance of the coating. It protects the underlying polymer paint layer from damage by forming a very fine, uniform and very hard mesh structure on the surface of the coating. It also has the characteristics of high hardness, high melting point, high wear resistance, corrosion resistance and excellent insulation properties. When added to floor coatings, it forms a hard and wear-resistant coating that can effectively protect the coated surface from wear and damage, thereby improving the durability and impact resistance of the coating.

[0024] Beneficial effects of the present invention:

[0025] 1. Compared with the prior art, the present invention adds talcum powder as a filler into polyurethane, and uses isopropyl triisostearate titanate to modify the surface of talcum powder. The monoalkoxy titanate coupling agent can be directly coupled with the trace hydroxyl groups adsorbed on the surface of talcum powder through the alkoxy group, thereby enhancing the interaction between talcum powder and polyurethane matrix, and significantly inhibiting the formation of stress concentration points around talcum powder particles. When added to polyurethane floor coating, the dispersion is more uniform and dense, and the stress concentration generated at the cracks when the coating film is subjected to stress is effectively dispersed, thereby effectively improving the tensile strength and wear resistance of the coating film.

[0026] 2. Compared with the prior art, the present invention compounds single-walled carbon nanotubes with mesoporous silica to achieve a synergistic effect. First, ethyl silicate is used as a precursor to obtain silica gel, single-walled carbon nanotubes are added to the silica gel to obtain single-walled carbon nanotube gel, and then the single-walled carbon nanotube gel is added to the synthesized mesoporous silica. The mesoporous silica can be used as a carrier of single-walled carbon nanotubes to obtain an antistatic material component B with good dispersibility and not easy to agglomerate. After modification, the surface of the antistatic material particles has a layer of silica gel composite film, which further reduces the friction coefficient and thus inhibits and reduces the generation of static charge. At the same time, the silica gel wraps the antistatic material and then ultrasonically disperses it. The gel on the surface of the particles slowly polymerizes between the aged colloid particles, promoting a dense three-dimensional Si-O-Si network, and then added to the organic polyurethane and the solution. Compared with a single single-walled carbon nanotube or mesoporous silica particles, the stability and dispersibility are improved. DETAILED DESCRIPTION

[0027] The parameters of the specific chemical substances used in the examples are from the following sources:

[0028] Water-based polyurethane resin: translucent liquid with a solid content of 32%. The manufacturer is Shenzhen Yoshida Chemical Co., Ltd., and the model is F0410.

[0029] Talc powder: particle size is 45μm, manufacturer is Dongguan Jinxin Powder Technology Co., Ltd., model is No. 2.

[0030] TY-1699: Suitable for water-based polyurethane and water. The manufacturer is Jining Fangyu Chemical Co., Ltd.

[0031] BYK-110: light yellow liquid, solid content is 52%, the manufacturer is Guangzhou Dachuan Fine Chemical Co., Ltd.

[0032] Single-walled carbon nanotubes: diameter is 20-40nm, length is 1-2μm, manufacturer is Shanghai Yuanye Biotechnology Co., Ltd., model number is T19281.

[0033] Titanium dioxide: The average particle size is 0.21 μm, the brand is ISK, and the model is TIPAQUE CR-60-2.

[0034] Nano-alumina: The average particle size is 30-60nm, the specific surface area is 10-30m2 / g, the manufacturer is Xuancheng Jingrui New Materials Co., Ltd., and the model is VK-L30H.

[0035] Example 1

[0036] A method for preparing a polyurethane antistatic and ultra-wear-resistant floor coating comprises the following steps:

[0037] (1) 5 g of isopropyl triisostearate titanate was added to 5 g of liquid paraffin and dispersed for 10 minutes, then added to 120 g of talc and stirred at 95° C. for 10 minutes, cooled to room temperature and added to 650 g of waterborne polyurethane resin and stirred for 0.5 hour, then 6 g of TY-1699, 10 g of BYK-110, 6 g of dimethyl silicone oil and 200 g of titanium dioxide were added and mixed and dispersed for 30 minutes, and ground with a sand mill to a fineness of 50 μm to obtain component A;

[0038] (2) Add 900 g of component A, 140 g of single-walled carbon nanotubes, and 100 g of nano-alumina to 400 parts of water, stir at room temperature at a rate of 1000 r / min for 0.5 hour, and filter to obtain a polyurethane antistatic and super wear-resistant floor coating.

[0039] Example 2

[0040] A method for preparing a polyurethane antistatic and ultra-wear-resistant floor coating comprises the following steps:

[0041] (1) 5 g of isopropyl triisostearate titanate was added to 5 g of liquid paraffin and dispersed for 10 minutes, then added to 120 g of talc and stirred at 95° C. for 10 minutes, cooled to room temperature and added to 650 g of waterborne polyurethane resin and stirred for 0.5 hour, then 6 g of TY-1699, 10 g of BYK-110, 6 g of dimethyl silicone oil and 200 g of titanium dioxide were added and mixed and dispersed for 30 minutes, and ground with a sand mill to a fineness of 50 μm to obtain component A;

[0042] (2) 160 g of ethyl silicate was added to 1500 g of anhydrous ethanol, and 1200 g of water was added to dilute it. The pH value was adjusted to 4 with 37 wt.% hydrochloric acid, and the mixture was stirred at room temperature for 3 hours. The mixture was ultrasonically treated at 25 W for 1 hour to obtain silica gel. 60 g of single-walled carbon nanotubes was added, and the mixture was stirred for another hour to obtain single-walled carbon nanotube-gel for later use.

[0043] (3) Add 900 g of component A, 140 g of single-walled carbon nanotube-gel, and 100 g of nano-alumina to 400 parts of water, stir at room temperature at a rate of 1000 r / min for 0.5 hour, and filter to obtain a polyurethane antistatic and super wear-resistant floor coating.

[0044] Example 3

[0045] A method for preparing a polyurethane antistatic and ultra-wear-resistant floor coating comprises the following steps:

[0046] (1) 5 g of isopropyl triisostearate titanate was added to 5 g of liquid paraffin and dispersed for 10 minutes, then added to 120 g of talc and stirred at 95° C. for 10 minutes, cooled to room temperature and added to 650 g of waterborne polyurethane resin and stirred for 0.5 hour, then 6 g of TY-1699, 10 g of BYK-110, 6 g of dimethyl silicone oil and 200 g of titanium dioxide were added and mixed and dispersed for 30 minutes, and ground with a sand mill to a fineness of 50 μm to obtain component A;

[0047] (2) 160 g of ethyl silicate was added to 1500 g of anhydrous ethanol, and 1200 g of water was added to dilute it. The pH value was adjusted to 4 with 37 wt.% hydrochloric acid, and the mixture was stirred at room temperature for 3 hours. The mixture was ultrasonically treated at 25 W for 1 hour to obtain silica gel. 60 g of single-walled carbon nanotubes was added, and the mixture was stirred for another hour to obtain single-walled carbon nanotube-gel for later use.

[0048] (3) Add 120 g of 30 wt.% sodium hydroxide aqueous solution to 4000 g of water and stir at room temperature for 10 minutes, add 120 g of single-walled carbon nanotube-gel, 150 g of water, and 150 g of 6 wt.% hexadecyltrimethylammonium bromide aqueous solution, disperse at 25W ultrasonic dispersion for 10 minutes, stir at 80°C for 1 hour, add 60 g of ethyl silicate at 80°C, react at 80°C for 6 hours, cool to room temperature and filter, wash the filter cake with water and filter, wash the filter cake with methanol and filter, repeat the methanol washing and filtering operation 4 times, and dry at 60°C for 2 hours to obtain component B;

[0049] (4) Add 900 g of component A, 140 g of component B, and 100 g of nano-alumina to 400 parts of water, stir at room temperature at a rate of 1000 r / min for 0.5 hour, and filter to obtain a polyurethane antistatic and super wear-resistant floor coating.

[0050] Example 4

[0051] A method for preparing a polyurethane antistatic and ultra-wear-resistant floor coating comprises the following steps:

[0052] (1) Add 120 g of talc to 650 g of waterborne polyurethane resin and stir for 0.5 hour, then add 6 g of TY-1699, 10 g of BYK-110, 6 g of dimethyl silicone oil and 200 g of titanium dioxide and mix and disperse for 30 minutes, and grind with a sand mill to a fineness of 50 μm to obtain component A;

[0053] (2) 160 g of ethyl silicate was added to 1500 g of anhydrous ethanol, and 1200 g of water was added to dilute it. The pH value was adjusted to 4 with 37 wt.% hydrochloric acid, and the mixture was stirred at room temperature for 3 hours. The mixture was ultrasonically treated at 25 W for 1 hour to obtain silica gel. 60 g of single-walled carbon nanotubes was added, and the mixture was stirred for another hour to obtain single-walled carbon nanotube-gel for later use.

[0054] (3) Add 120 g of 30 wt.% sodium hydroxide aqueous solution to 4000 g of water and stir at room temperature for 10 minutes, add 120 g of single-walled carbon nanotube-gel, 150 g of water, and 150 g of 6 wt.% hexadecyltrimethylammonium bromide aqueous solution, disperse at 25W ultrasonic dispersion for 10 minutes, stir at 80°C for 1 hour, add 60 g of ethyl silicate at 80°C, react at 80°C for 6 hours, cool to room temperature and filter, wash the filter cake with water and filter, wash the filter cake with methanol and filter, repeat the methanol washing and filtering operation 4 times, and dry at 60°C for 2 hours to obtain component B;

[0055] (4) Add 900 g of component A, 140 g of component B, and 100 g of nano-alumina to 400 parts of water, stir at room temperature at a rate of 1000 r / min for 0.5 hour, and filter to obtain a polyurethane antistatic and super wear-resistant floor coating.

[0056] Test Example 1

[0057] The polyurethane antistatic and ultra-wear-resistant floor coating obtained in Examples 1-4 was applied to one side of a concrete substrate with a size of 100mm×100mm×40mm by a brush coating method, and the dry film thickness was 1mm to obtain the test panels of Examples 1-4, 3 panels in each group, and the wear resistance test was performed after curing at 25°C and 50% humidity for 5 days; the coating surface should be smooth and flat, without obvious defects such as bubbles and cracks. The test steps were tested in accordance with the national standard GB / T 22374-2018 "Determination of wear resistance-rotating rubber grinding wheel method" for floor coating materials.

[0058] Fix the test plate on the turntable, lower the friction head and place the rubber grinding wheel on the surface of the test plate. The rubber grinding wheel model is CS-17. Place the dust suction nozzle and adjust the position of the dust suction nozzle so that it is 1mm away from the surface of the wafer; turn on the dust suction device and then start the turntable, run the rubber grinding wheel on the test plate for 100 revolutions, remove any loose grinding chips remaining on the test plate with lint-free paper, weigh the test plate again, and check the test plate to see if the coating is worn through; repeat the above steps on the other two test plates and record the results, and take the average value of the test data.

[0059] The mass of the test plate before the test was weighed to an accuracy of 0.1 mg and recorded as the initial mass; after the test, the average mass loss of the three test plates in the same group was calculated using the reduction method to an accuracy of 1 mg. The test data is shown in Table 1.

[0060] Table 1 Wear resistance test data

[0061] Example 1 Example 2 Example 3 Example 4 Average mass loss / g 0.028g 0.024g 0.010g 0.018g

[0062] Through test example 1, the coating film of the floor coating in Example 1 on the concrete substrate, the antistatic material is carbon nanotubes added separately, the nanoparticles are easy to agglomerate, resulting in a slightly reduced wear resistance; the coating film of the floor coating on the concrete substrate in Example 2, carbon nanotubes are added to the silica gel, which solves the dispersion problem to a certain extent; the coating film of the floor coating on the concrete substrate in Example 3, the carbon nanotube-gel is adsorbed on the mesoporous silica carrier, the dispersion is uniform, the mass loss is minimal, and the wear resistance is best; Example 4 is used as a comparison with Example 3, talcum powder is directly added as a filler, the stress concentration is caused in the coating film, resulting in a reduction in wear resistance.

[0063] Test Example 2

[0064] The polyurethane antistatic and ultra-wear-resistant floor coating obtained in Examples 1-4 was applied to one side of a concrete substrate with a size of 1.2m×1.2mm×40mm by brush coating to obtain the test specimens of Examples 1-4. The dry film thickness was 4mm. The test was conducted after being placed at 25°C and 30% humidity for 24 hours. The coating surface should be flat and crack-free. The test procedure was carried out in accordance with the industry standard SJ / T11294-2018 "General Specification for Antistatic Floor Coatings". The antistatic performance of the antistatic floor is specified as follows: the point-to-point resistance is 5.0×10 4 Ω~1.0×10 9 Ω, it complies with industry standards.

[0065] The sample was placed on a smooth and flat ground for testing. The ground was used as a test platform to ensure that the floor sample had a ground terminal connected to the ground. When a voltage of 500 V was applied to the platform, the point-to-point resistance of the platform was greater than 1.0×10 13 Ω. Connect two columnar electrodes to the instrument, place the sample on the test platform with the surface facing upward, place the two electrodes on the surface of the sample, and keep the longitudinal test distance of the electrodes at 300mm; connect one end of the test instrument to the ground terminal of the sample, and the other end to the columnar electrode; load the instrument with a 10.0V test voltage, and record the surface resistance reading after 15s; if the resistance reading is less than 1.0×10 6 Ω, record the result; if the resistance value is equal to or greater than 1.0×10 6 Ω, unload the instrument, reload the 100.0V test voltage, repeat the above steps and record the measurement results; the readings are rounded to one decimal place, and each group is repeated 5 times. The test data are shown in Table 2.

[0066] Table 2 Antistatic performance test data

[0067] Example 1 Example 2 Example 3 Example 4 Surface resistance / Ω <![CDATA[1.5×10 6 ]]> <![CDATA[3.5×10 6 ]]> <![CDATA[2.2×10 8 ]]> <![CDATA[1.8×10 8 ]]>

[0068] By comparing with Test Example 2, it can be seen that the poor dispersibility and easy agglomeration of carbon nanotubes in antistatic materials will affect the better performance of antistatic materials. In Example 1, the floor coating on the concrete substrate has a coating of carbon nanotubes added separately; in Example 2, the floor coating on the concrete substrate has carbon nanotubes added to the silica gel and then added to the coating; in Example 3, the floor coating on the concrete substrate has the carbon nanotube-gel adsorbed on the mesoporous silica carrier, which has the best dispersion effect and the most comprehensive effect; Example 4 is used as a comparison with Example 3, and talcum powder is directly added as a filler without modifying the talcum powder. The dispersibility of the talcum powder only slightly affects the dispersibility of the antistatic material, and the antistatic performance is slightly lower than that of Example 3.

Claims

1. A method for preparing a polyurethane antistatic and ultra-wear-resistant floor coating, characterized in that: The following steps are involved: (1) adding isopropyl titanate triisostearate to liquid paraffin for dispersion, adding talcum powder for stirring, cooling to room temperature, adding to polyurethane for stirring, then adding a wetting agent, a dispersant, a defoaming agent, and a pigment for mixing and dispersion, and grinding with a sand mill to obtain component A; (2) adding ethyl silicate to anhydrous ethanol, adding water to dilute, adjusting the pH value to acidic with hydrochloric acid, stirring at room temperature, and ultrasonic treatment to obtain silica gel, adding single-walled carbon nanotubes and continuing to stir to obtain single-walled carbon nanotube-gel for standby use; (3) adding sodium hydroxide aqueous solution to water and stirring at room temperature, adding single-walled carbon nanotube-gel, water, and hexadecyltrimethylammonium bromide aqueous solution, stirring after ultrasonic dispersion, adding ethyl silicate to react, filtering, washing the filter cake with water and filtering, washing the filter cake with methanol and filtering, repeating the methanol washing and filtering operation 4-6 times, and drying to obtain component B; (4) Add component A, component B and nano-alumina to water, stir at room temperature, and filter to obtain a polyurethane antistatic and super wear-resistant floor coating.

2. The method for preparing the polyurethane antistatic super wear-resistant floor coating according to claim 1, characterized in that: The grinding in step (1) is performed to a fineness of 40-50 μm.

3. The method for preparing the polyurethane antistatic super wear-resistant floor coating according to claim 1, characterized in that: The polyurethane in step (1) is a waterborne polyurethane resin.

4. The method for preparing the polyurethane antistatic super wear-resistant floor coating according to claim 1, characterized in that: The wetting agent in step (1) is an organosilicon wetting agent.

5. The method for preparing the polyurethane antistatic super wear-resistant floor coating according to claim 1, characterized in that: In the step (1), the dispersant is any one of BYK-110, BYK-190, BYK-161 and BYK-163.

6. The method for preparing the polyurethane antistatic super wear-resistant floor coating according to claim 1, characterized in that: The defoaming agent in step (1) is dimethyl silicone oil.

7. The method for preparing the polyurethane antistatic super wear-resistant floor coating according to claim 1, characterized in that: The sodium hydroxide aqueous solution in step (3) is a 10-30 wt. % sodium hydroxide aqueous solution.

8. A polyurethane antistatic and ultra-wear-resistant floor coating, characterized in that: The method is prepared by the method according to any one of claims 1 to 7.

9. An application of polyurethane antistatic super wear-resistant floor coating, characterized in that: The coating can be obtained by coating the polyurethane antistatic and super wear-resistant floor coating as described in claim 8 on a floor substrate.

10. The use according to claim 9, characterized in that The floor substrate is any one of a concrete substrate, a mortar substrate, a wood substrate and a metal substrate.

Citation Information

Patent Citations

  • Antistatic nano polyurethane floor paint

    CN106398504A

  • Special antistatic super-wear-resistant thin-layer material for ground of gas station and oil depot as well as construction method

    CN112431377A

  • Preparation method of mesoporous silicon-dioxide-coated single-wall carbon nanotubes

    CN104030294A

  • Heavy duty anticorrosive coating containing graphene and preparation method of same