Three-dimensional conductive agent, positive electrode sheet and electrochemical device

By using the three-dimensional conductive agent formed by cross-linking of carbon nanowires with loaded metal element, the charge transport dynamics and processing performance problems caused by the increase of the positive electrode sheet density is solved, and more efficient charge transport and a more stable pole sheet structure is achieved.

CN118263444BActive Publication Date: 2024-11-29三一红象电池有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410382640.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-29
Publication Date
2024-11-29
Estimated Expiration
2044-03-29

AI Technical Summary

Technical Problem

In the lithium-ion battery industry, the increase in the positive electrode plate surface density leads to a longer ion diffusion path, deterioration of charge transport kinetics, and deterioration of processing performance, and traditional carbon black and carbon nanotubes are difficult to meet the charge transport needs of thick electrode sheets.

Method used

The carbon nanowires loaded with metal element are cross-linked by silane coupling agent to form a three-dimensional conductive agent with a three-dimensional cross-linking network structure, which improves the charge transport dynamics of the thick electrodes, and increases the stability and processing performance of the electrode sheet through the three-dimensional framework structure. .

Benefits of technology

The charge transfer rate of thick electrodes is improved, the occurrence of lithium dendrites is reduced, the mechanical processing performance of thick electrode sheets is enhanced, cracking problems is avoided, and the overall performance of the electrochemical device is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118263444B_ABST
    Figure CN118263444B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of conductive agents, and specifically to a three-dimensional conductive agent, a positive electrode sheet, and an electrochemical device. The three-dimensional conductive agent includes a carbon nanonet having a three-dimensional cross-linked network structure, and the carbon nanonet is a carbon nanonet formed by cross-linking a metal-loaded carbon nanowire through a silane coupling agent. The three-dimensional conductive agent of the present invention can increase the charge transfer rate of thick electrodes, reduce lithium dendrites caused by excessive local current density, and the three-dimensional cross-linked network structure can relieve the stress accumulated inside the electrode sheet and increase the mechanical processing performance of the thick electrode sheet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of conductive agents, and in particular to three-dimensional conductive agents, positive electrode sheets and electrochemical devices. Background Art

[0002] At present, the conductive agents used in most positive electrode sheets during homogenization are conductive carbon black and carbon nanotubes. When the active material loaded on the electrode sheet is small, that is, when the surface density of the positive electrode is low, the conductive carbon black and carbon nanotubes used can meet the requirements of the electrode sheet for charge transfer dynamics under the action of the binder. As the competition in the lithium-ion battery industry becomes increasingly fierce, reducing the cost of battery cells to improve the competitiveness of products has become an inevitable development trend. Increasing the amount of active material loaded on the positive electrode sheet, that is, increasing the surface density of the electrode sheet, can reduce the amount of current collector used and achieve the purpose of cost reduction.

[0003] However, the increase in the pole piece surface density makes the pole piece thicker, which will lead to a longer ion diffusion path, worse charge transfer dynamics and worse processing performance, resulting in poor rate performance of thick pole pieces, easy lithium precipitation during high rate discharge, and easy cracking of thick pole pieces during baking. At this time, the carbon black and carbon nanotubes used in thin pole pieces are difficult to meet the charge transfer dynamics requirements of thick pole pieces in space. Summary of the invention

[0004] In view of this, the present invention provides a three-dimensional conductive agent, a positive electrode sheet and an electrochemical device. The three-dimensional conductive agent can improve the charge transfer kinetics of thick electrodes, and the three-dimensional skeleton structure can increase the stability of the electrode sheet and improve the processing performance of the thick electrode sheet.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] In a first aspect, the present invention provides a three-dimensional conductive agent, which includes a carbon nanonet having a three-dimensional cross-linked network structure, wherein the carbon nanonet is a carbon nanonet formed by cross-linking carbon nanowires loaded with metal elements through a silane coupling agent.

[0007] In the embodiment of the present invention, the silane coupling agent includes but is not limited to vinyl trimethoxy silane (CAS No. 2768-02-7), vinyl triethoxy silane (CAS No. 78-08-0), dodecyl trimethoxy silane (CAS No. 3069-21-4), dodecyl triethoxy silane (CAS No. 18536-91-9), hexadecyl trimethoxy silane (CAS No. 16415-12-6), hexadecyl triethoxy silane (CAS No. 16415-13-7), phenyl trimethoxy silane (CAS No. 2996-92-1), γ-aminopropyl trimethoxy silane (CAS No. 13822-56-5), 3 - At least one of glycidyloxypropyltrimethoxysilane (CAS No. 2530-83-8), γ-methacryloxypropyltrimethoxysilane (CAS No. 2530-85-0), N-β-aminoethyl-γ-aminopropyltriethoxysilane (CAS No. 5089-72-5), methoxytriethylene glycol ether propyltrimethoxysilane (CAS No. 132388-45-5), 11-mercaptoundecyltrimethoxysilane (CAS No. 877593-17-4), 3-mercaptopropyltrimethoxysilane (CAS No. 4420-74-0), and diethylphosphoethyltriethoxysilane (CAS No. 757-44-8).

[0008] Preferably, the metal element includes at least one of aluminum (Al), silver (Ag), and gold (Au).

[0009] In a second aspect, the present invention provides a method for preparing the above three-dimensional conductive agent, comprising the following steps:

[0010] Dissolving nanocellulose and metal salt in water, filtering out solids after first ultrasonic stirring, and then drying to obtain powder;

[0011] In an inert atmosphere, the powder is carbonized to obtain carbon nanowires loaded with metal elements;

[0012] The carbon nanowire loaded with metal element and the silane coupling agent are dissolved in an organic solvent, and after a second ultrasonic stirring, a three-dimensional conductive agent is obtained.

[0013] Preferably, the mass percentage of the metal salt to the nanocellulose is 5% to 15%.

[0014] Preferably, the mass percentage of the silane coupling agent to the carbon nanowires loaded with metal element is 1% to 3%.

[0015] Preferably, the first ultrasonic stirring or the second ultrasonic stirring lasts for 10 to 30 minutes and has a frequency of 1.6 to 1.8 KHz.

[0016] Preferably, the carbonization temperature is 1100-1300° C. and the time is 4-6 hours.

[0017] In a third aspect, the present invention provides a positive electrode sheet, the positive electrode sheet comprising a positive electrode current collector, and a positive electrode active material layer disposed on at least one side surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material, a conductive agent and a binder;

[0018] The conductive agent includes a first conductive agent, or includes a first conductive agent and a second conductive agent;

[0019] The first conductive agent is the three-dimensional conductive agent mentioned above;

[0020] The second conductive agent includes at least one of carbon black, carbon nanotubes, graphene, and acetylene black.

[0021] Preferably, the coating surface density of the positive electrode active material layer is 400 to 700 g / m 2 .

[0022] Preferably, the mass percentage of the first conductive agent to the total mass of the conductive agent is 30% to 100%.

[0023] In a fourth aspect, the present invention provides an electrochemical device, which includes the above-mentioned positive electrode sheet.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] In the present invention, carbon nanowires loaded with high-conductivity metal elements are cross-linked through a silane coupling agent to form a three-dimensional cross-linked network structure. On the one hand, the highly conductive carbon nanowire can increase the charge transfer rate of the thick electrode and reduce lithium dendrites caused by excessive local current density; on the other hand, the three-dimensional cross-linked network structure has a certain mechanical strength. During the baking process of the thick electrode, the cross-linked conductive network skeleton can relieve the stress accumulated inside the electrode due to uneven solvent volatilization, increase the mechanical processing performance of the thick electrode, and thus alleviate the processing problem of cracking of the thick electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is an electron microscope photo of the three-dimensional conductive agent of the present invention;

[0027] Figure 2 It is a schematic diagram of the structure of the three-dimensional conductive agent of the present invention;

[0028] Figure 3 It is a schematic diagram of the cross-sectional structure of carbon nanowires loaded with metal elements in the three-dimensional conductive agent of the present invention;

[0029] Figure 4 The present invention is a flow chart of the preparation of the three-dimensional conductive agent and the homogenous coating of the positive electrode slurry. DETAILED DESCRIPTION

[0030] The present invention discloses a three-dimensional conductive agent, a positive electrode sheet and an electrochemical device. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0031] In order to improve the charge transfer kinetics of thick electrodes and alleviate the processing problem of thick electrode cracking, the present invention provides a three-dimensional conductive agent, a positive electrode sheet and an electrochemical device. The specific technical solution is as follows:

[0032] In a first aspect, the present invention provides a three-dimensional conductive agent, which includes a carbon nanonet having a three-dimensional cross-linked network structure, wherein the carbon nanonet is a carbon nanonet formed by cross-linking carbon nanowires loaded with metal elements through a silane coupling agent.

[0033] In the present invention, the surface of the carbon nanowire loaded with metal elements and its surface bound water contain hydroxyl groups, the silane coupling agent reacts with the surface hydroxyl groups to form silicon-oxygen bonds, and the carbon nanowires loaded with metal elements are cross-linked to form a carbon nanonet. The continuous three-dimensional conductive network can improve the charge transfer dynamics of the thick electrode in space, uniform the current density in space, and reduce the safety problem of lithium dendrite growth caused by excessive polarization.

[0034] In the embodiment of the present invention, the silane coupling agent includes but is not limited to at least one of vinyl trimethoxysilane, vinyl triethoxysilane, dodecyl trimethoxysilane, dodecyl triethoxysilane, hexadecyl trimethoxysilane, hexadecyl triethoxysilane, phenyl trimethoxysilane, γ-aminopropyl trimethoxysilane, 3-glycidyl ether oxypropyl trimethoxysilane, γ-methacryloxypropyl trimethoxysilane, N-β-aminoethyl-γ-aminopropyl triethoxysilane, methoxy triethylene glycol ether propyl trimethoxysilane, 11-mercapto undecyl trimethoxysilane, 3-mercaptopropyl trimethoxysilane, and diethylphosphoethyl triethoxysilane. As long as the type of silane coupling agent recognized by those skilled in the art is within the protection scope of the present invention.

[0035] In the process of preparing the three-dimensional conductive network skeleton, a metal element with high conductivity is loaded on the skeleton to improve the conductivity of the entire skeleton. Preferably, the metal element includes at least one of aluminum (Al), silver (Ag), and gold (Au).

[0036] In a second aspect, the present invention provides a method for preparing the above three-dimensional conductive agent, comprising the following steps:

[0037] Dissolving nanocellulose and metal salt in water, filtering out solids after first ultrasonic stirring, and then drying to obtain powder;

[0038] In an inert atmosphere, the powder is carbonized to obtain carbon nanowires loaded with metal elements;

[0039] The carbon nanowire loaded with metal element and the silane coupling agent are dissolved in an organic solvent, and after a second ultrasonic stirring, a three-dimensional conductive agent is obtained.

[0040] In the above preparation method, nanocellulose is carbonized and reduced at high temperature to generate low-graphitized carbon nanowires, and metal salt is carbonized and reduced at high temperature to generate metal elements with high conductivity.

[0041] Preferably, the mass percentage of the metal salt to the nanocellulose is 5% to 15%. Exemplarily, the mass percentage of the metal salt to the nanocellulose is any value among 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, or any value in the range consisting of any two of the above values.

[0042] Preferably, the mass percentage of the silane coupling agent to the carbon nanowires loaded with metal elements is 1% to 3%. Exemplarily, the mass percentage of the silane coupling agent to the carbon nanowires loaded with metal elements is 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.6%, 2.8%, 3%, or any value in the range of any two of the above values.

[0043] In an embodiment of the present invention, in the method for preparing the three-dimensional conductive agent, the mass ratio of the metal salt, nanocellulose and water is (5-15):100:(100-1000).

[0044] In an embodiment of the present invention, the mass ratio of the silane coupling agent, the carbon nanowires loaded with metal elements, and the organic solvent is (1-3):100:(100-1000).

[0045] In an embodiment of the present invention, the nanocellulose has a length of 0.5 to 5 μm and a diameter of 1 to 100 nm.

[0046] In a specific embodiment of the present invention, the nanocellulose has a length of 1 to 3 μm and a diameter of 3 to 50 nm.

[0047] In an embodiment of the present invention, the metal salt includes at least one of aluminum salt (Al salt), silver salt (Ag salt), and gold salt (Au salt). Exemplarily, the metal salt includes but is not limited to at least one of aluminum sulfate, aluminum chloride, aluminum nitrate, silver sulfate, silver chloride, silver nitrate, and gold chloride.

[0048] Preferably, the time of the first ultrasonic stirring or the second ultrasonic stirring is 10 to 30 minutes, and the frequency is 1.6 to 1.8 kHz. The time of the first ultrasonic stirring or the second ultrasonic stirring is exemplarily any value in 10 minutes, 12 minutes, 14 minutes, 16 minutes, 18 minutes, 20 minutes, 22 minutes, 24 minutes, 26 minutes, 28 minutes, 30 minutes, or any value in the range of any two of the above values. The frequency of the first ultrasonic stirring or the second ultrasonic stirring is exemplarily any value in 1.6 kHz, 1.65 kHz, 1.7 kHz, 1.75 kHz, 1.8 kHz, or any value in the range of any two of the above values.

[0049] Preferably, the carbonization temperature is 1100-1300°C, and the time is 4-6h. The carbonization temperature is exemplarily any one of 1100°C, 1150°C, 1200°C, 1250°C, 1300°C, or any one of the ranges consisting of any two of the above values. The carbonization time is exemplarily any one of 4h, 4.5h, 5h, 5.5h, 6h, or any one of the ranges consisting of any two of the above values.

[0050] In a third aspect, the present invention provides a positive electrode sheet, the positive electrode sheet comprising a positive electrode current collector, and a positive electrode active material layer disposed on at least one side surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material, a conductive agent and a binder;

[0051] In an embodiment of the present invention, the conductive agent includes a first conductive agent, or includes a first conductive agent and a second conductive agent, the first conductive agent is the above-mentioned three-dimensional conductive agent, and the second conductive agent includes but is not limited to at least one of carbon black, carbon nanotubes, graphene, and acetylene black.

[0052] Preferably, the coating surface density of the positive electrode active material layer is 400 to 700 g / m 2 The coating surface density of the positive electrode active material layer is 400 g / m 2 , 500g / m 2 , 600g / m 2 , 700g / m 2 Any value in the range or any value in the range consisting of any two of the above values.

[0053] Preferably, the mass percentage of the first conductive agent to the total mass of the conductive agent is 30% to 100%. The mass percentage of the first conductive agent to the total mass of the conductive agent is exemplarily any value among 30%, 40%, 50%, 60%, 70%, 80%, 90%, 100%, or any value in the range of any two of the above values.

[0054] In the embodiment of the present invention, the mass percentage of each component in the positive electrode active material layer is: positive electrode active material 70% to 90%, conductive agent 5% to 15%, and binder 5% to 15%.

[0055] The present invention also provides a method for preparing the positive electrode sheet, comprising the following steps:

[0056] The positive electrode active material, the conductive agent, the binder and the first solvent are mixed to obtain a positive electrode slurry; the conductive agent includes a first conductive agent, or includes a first conductive agent and a second conductive agent, the first conductive agent is the above-mentioned three-dimensional conductive agent, and the second conductive agent includes but is not limited to at least one of carbon black, carbon nanotubes, graphene and acetylene black;

[0057] The positive electrode slurry is coated on at least one side of the positive electrode current collector, and after drying and rolling, a positive electrode sheet is obtained.

[0058] In the above preparation method, coating, drying and rolling are all conventional means and will not be described in detail in the present invention.

[0059] The present invention also provides another method for preparing the above-mentioned positive electrode sheet, comprising the following steps:

[0060] The positive electrode active material, the conductive agent, the binder and the first solvent are mixed to obtain a positive electrode slurry; the conductive agent includes a first conductive agent, or includes a first conductive agent and a second conductive agent, the first conductive agent is the above-mentioned three-dimensional conductive agent, and the second conductive agent includes but is not limited to at least one of carbon black, carbon nanotubes, graphene and acetylene black;

[0061] The positive electrode slurry is coated on at least one side of the positive electrode current collector, and after cold pressing, cutting and drying, a positive electrode sheet is obtained.

[0062] In the above preparation method, the processes of coating, cold pressing, cutting and drying are all conventional means and will not be described in detail in the present invention.

[0063] In a fourth aspect, the present invention provides an electrochemical device, which includes the above-mentioned positive electrode sheet.

[0064] In an embodiment of the present invention, the electrochemical device is a battery. The battery may be a secondary battery or a primary battery, preferably a secondary battery. For example, the battery may be a lithium ion secondary battery, a lithium primary battery, a sodium ion battery, a magnesium ion battery, etc., but is not limited thereto. The battery structure of the present application includes but is not limited to a soft-pack lithium ion battery, a square hard-shell battery or a cylindrical hard-shell battery, etc. It should be noted that in a specific embodiment, the present application is explained using a lithium ion battery as an example of a secondary battery, but the battery of the present application is not limited to a lithium ion battery.

[0065] The battery can be a button cell prepared by using a conventional lamination process to prepare the above-mentioned positive electrode sheet and the conventional negative electrode sheet according to the button cell assembly requirements; the battery can also be a lithium-ion secondary battery prepared by using a conventional lamination process or a winding process to prepare the above-mentioned positive electrode sheet and the conventional negative electrode sheet together into a bare cell, and then assembling a protection circuit and a shell.

[0066] In an embodiment of the present invention, the electrochemical device further includes a negative electrode sheet, a separator and an electrolyte.

[0067] In an embodiment of the present invention, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one side surface of the negative electrode current collector.

[0068] In an embodiment of the present invention, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material can be a negative electrode active material for a battery known in the art. The present application does not particularly limit the type of negative electrode active material, as long as the purpose of the present application can be achieved. As an example, the negative electrode active material may include at least one of the following materials: natural graphite, artificial graphite, soft carbon, hard carbon, mesophase carbon microspheres, silicon-based materials, tin-based materials, lithium titanate, transition metal nitrides, etc. The above-mentioned silicon-based material can be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites and silicon alloys. The tin-based material can be selected from at least one of elemental tin, tin oxide compounds and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries can also be used. These negative electrode active materials can be used alone or in combination of two or more.

[0069] In an embodiment of the present invention, the negative electrode active material layer further includes at least one of a conductive agent, a binder, and a thickener. The present application does not particularly limit the types of conductive agents, binders, and thickeners in the negative electrode active material layer, as long as the purpose of the present application can be achieved. As an example, the conductive agent in the negative electrode active material layer can be selected from at least one of acetylene black, conductive carbon black, Ketjen black, carbon nanotubes, graphene, and carbon nanofibers. As an example, the binder in the negative electrode active material layer can be selected from at least one of carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), polymethacrylic acid (PMAA), carboxymethyl chitosan (CMCS), and sodium alginate (SA). As an example, the thickener in the negative electrode active material layer can be selected from at least one of polyvinyl alcohol and its modified bodies, starch and its modified bodies, cellulose derivatives, polyvinyl pyrrolidone, polyacrylic acid (salt), and polyethylene glycol.

[0070] The present application has no particular restrictions on the mass ratio of the negative electrode active material, the conductive agent, the binder and the thickener in the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the mass percentage of each component in the negative electrode active material layer is: 70% to 97% of the negative electrode active material, 1% to 10% of the conductive agent, 1% to 10% of the binder, and 1% to 10% of the thickener.

[0071] The present application has no particular restrictions on the organic solvent, electrolyte salt, and additives in the electrolyte, and those skilled in the art can select them according to actual needs as long as the purpose of the present application can be achieved.

[0072] In an embodiment of the present invention, the electrolyte salt is a lithium salt, and the lithium salt may include a combination of one or more of lithium bis(fluorosulfonyl)imide (LiFSI), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium bis(oxalatoborate) (LiBOB), lithium difluorophosphate (LiPO2F2), lithium tetrafluorooxalate phosphate (LiTFOP), etc. The concentration of the lithium salt may be 0.5 to 3.0 mol / L.

[0073] In an embodiment of the present invention, the organic solvent may include one or more combinations of ethylene carbonate (EC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl formate (MF), methyl acetate (MA), fluoroethylene carbonate (FEC), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), cyclopentane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS), diethyl sulfone (ESE), etc.

[0074] However, the present application is not limited to the above-mentioned lithium salts and organic solvents. The present application may also use other traditional substances that can be used as lithium salts and organic solvents in battery electrolytes.

[0075] In an embodiment of the present invention, additives in the electrolyte may or may not be added. The additives in the electrolyte may include film-forming additives, and may also include additives that can improve certain properties of the battery, such as additives that improve the overcharge performance of the battery, additives that improve the high temperature or low temperature performance of the battery, etc. The embodiments of the present application do not particularly limit the additives in the electrolyte, and those skilled in the art can choose according to actual needs. Exemplarily, the additives include but are not limited to at least one of cyclic carbonate additives, cyclic sultone additives, nitrile additives or lithium salt additives. The mass percentage of the additives in the electrolyte may be less than or equal to 15%.

[0076] The present application has no particular limitation on the separator in the battery, and those skilled in the art can select it according to actual needs, as long as the purpose of the present application can be achieved.

[0077] In some embodiments, the material of the separator may include at least one of polyethylene, polypropylene, glass fiber, non-woven fabric, and polyvinylidene fluoride.

[0078] The diaphragm can be a single-layer film or a multi-layer composite film, without any particular limitation. When the diaphragm is a multi-layer composite film, the materials of each layer can be the same or different, without any particular limitation.

[0079] The reagents, instruments or materials used in the present invention can be obtained through commercial channels.

[0080] The present invention will be further described below in conjunction with embodiments:

[0081] Example 1

[0082] (I) Preparation of positive electrode

[0083] (1) Preparation of three-dimensional conductive agents

[0084] 100 g of nanocellulose with a length of 1 to 3 μm and a diameter of 3 to 50 nm was placed in 400 g of deionized water, and 5 g (equivalent to 5 wt% of the mass of the nanocellulose) of metal salt (aluminum sulfate) was added. The mixture was ultrasonically stirred and mixed at a frequency of 1.7 KHz for 10 min, and then filtered and dried.

[0085] The dried powder was placed in a tube furnace and carbonized at 1100° C. for 4 h under an inert atmosphere to obtain metal-loaded carbon nanowires X-CNF (wherein X represents metal and CNF represents carbon nanowires);

[0086] 100g of metal-loaded carbon nanowires were placed in 400g of N-methylpyrrolidone (NMP), and 1g (equivalent to 1wt% of the mass of the metal-loaded carbon nanowires) of silane coupling agent vinyltrimethoxysilane was added. After ultrasonic stirring and mixing at a frequency of 1.7KHz for 10min, the mixture was filtered and dried to obtain a three-dimensional conductive agent. The electron microscope photo is shown in FIG. Figure 1 The structural diagram is shown in Figure 2 and Figure 3 , the preparation flow chart is shown in Figure 4 The three-dimensional conductive agent is used as the first conductive agent in the subsequent preparation of the positive electrode sheet.

[0087] (2) Preparation of positive electrode

[0088] The positive electrode active material (lithium cobalt oxide), the first conductive agent (the three-dimensional conductive agent prepared above), the second conductive agent (carbon black), and the binder (PVDF) were mixed in a mass ratio of 8:0.5:0.5:1, and an appropriate amount of N-methylpyrrolidone (NMP) was added to prepare a positive electrode slurry. The positive electrode slurry was evenly coated on both sides of the aluminum foil surface with a coating surface density of 500 g / m 2 After drying and roller pressing, the positive electrode sheet is obtained.

[0089] (II) Preparation of negative electrode sheet

[0090] The negative electrode active material (artificial graphite), conductive agent (Super P), binder (styrene-butadiene rubber SBR), and thickener (polyvinyl pyrrolidone) were mixed in a mass ratio of 8:0.5:0.5:1, and an appropriate amount of deionized water was added to prepare the negative electrode slurry. The negative electrode slurry was evenly coated on both sides of the copper foil surface, and the double-sided coating surface density was 277.7g / m 2 After drying and roller pressing, the negative electrode sheet is obtained.

[0091] (III) Preparation of diaphragm

[0092] A polyethylene (PE) porous membrane with a thickness of 5 μm (provided by Celgard) was used.

[0093] (IV) Preparation of electrolyte

[0094] LiPF6 was dissolved in a solvent of ethylene carbonate, ethyl methyl carbonate and diethyl carbonate in a volume ratio of 1:1:1, and the concentration of LiPF6 was 1.2 mol / L.

[0095] (V) Preparation of lithium-ion batteries

[0096] The positive electrode sheet, separator and negative electrode sheet prepared above are stacked in order, so that the separator is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then wound to obtain an electrode assembly. After welding the pole ear, the electrode assembly is placed in an aluminum plastic film packaging shell, placed in an 85°C vacuum oven for 12 hours to remove moisture, and injected with electrolyte. After vacuum packaging, standing, formation (0.02C constant current charging to 3.5V, and then 0.1C constant current charging to 3.9V), shaping, capacity testing and other processes, a lithium-ion battery is obtained.

[0097] Example 2 Group

[0098] The other conditions of this embodiment group and embodiment 1 remain unchanged, except that the mass proportion of the metal salt is changed in the preparation of the three-dimensional conductive agent.

[0099] Example 2a: The mass of the metal salt is equivalent to 10 wt% of the mass of the nanocellulose;

[0100] Example 2b: The mass of the metal salt is equivalent to 15 wt% of the mass of the nanocellulose.

[0101] Example 3 Group

[0102] The other conditions of this embodiment group and embodiment 2a remain unchanged, except that the time of two ultrasonic stirrings is different in the preparation of the three-dimensional conductive agent.

[0103] Example 3a: The ultrasonic stirring time was 20 min for each of the two times;

[0104] Example 3b: The ultrasonic stirring time was 30 min for each of the two times.

[0105] Example 4 Group

[0106] The other conditions of this embodiment group and embodiment 3a remain unchanged, except that the carbonization temperature is different in the preparation of the three-dimensional conductive agent.

[0107] Example 4a: The carbonization temperature is 1200°C;

[0108] Example 4b: The carbonization temperature is 1300°C.

[0109] Example 5 Group

[0110] The other conditions of this embodiment group and embodiment 4b remain unchanged, except that the carbonization time is different in the preparation of the three-dimensional conductive agent.

[0111] Example 5a: The carbonization time is 5 h;

[0112] Example 5b: The carbonization time is 6 h.

[0113] Example 6 Group

[0114] The other conditions of this embodiment group and embodiment 5a remain unchanged, except that the amount of silane coupling agent used in the preparation of the three-dimensional conductive agent is different.

[0115] Example 6a: The amount of the silane coupling agent used is equivalent to 2 wt% of the mass of the carbon nanowires loaded with metal element;

[0116] Example 6b: The amount of the silane coupling agent used is equivalent to 3 wt % of the mass of the carbon nanowires loaded with metal element.

[0117] Example 7 Group

[0118] The other conditions of this embodiment group and embodiment 6a remain unchanged, except that in the preparation of the positive electrode sheet, the mass ratios of the positive electrode active material, the first conductive agent, the second conductive agent, and the binder are different.

[0119] Example 7a: The mass ratio of the positive electrode active material, the first conductive agent, the second conductive agent, and the binder is 8:1:0:1;

[0120] Example 7b: The mass ratio of the positive electrode active material, the first conductive agent, the second conductive agent, and the binder is 8:0.8:0.2:1;

[0121] Example 7c: The mass ratio of the positive electrode active material, the first conductive agent, the second conductive agent, and the binder is 8:0.3:0.7:1.

[0122] Example 8 Group

[0123] The other conditions of this embodiment group and embodiment 6a remain unchanged, the difference is that in the preparation of the positive electrode sheet, the coating surface density of the positive electrode sheet is different.

[0124] Example 8a: Coating surface density is 600 g / m 2 ;

[0125] Example 8b: Coating surface density is 700 g / m 2 ;

[0126] Example 8c: Coating surface density is 400 g / m 2 .

[0127] Example 9 Group

[0128] The other conditions of this embodiment group and embodiment 6a remain unchanged, the difference is that in the preparation of the positive electrode sheet, the types of metal salts and the types of metal elements are different.

[0129] Embodiment 9a: The metal salt is silver sulfate, and the metal element is silver (Ag);

[0130] Example 9b: The metal salt is gold chloride, and the metal element is gold (Au).

[0131] Example 10 Group

[0132] The other conditions of this embodiment group and embodiment 6a remain unchanged, except that the type of the second conductive agent is different in the preparation of the positive electrode sheet.

[0133] Embodiment 10a: The second conductive agent is carbon nanotubes;

[0134] Embodiment 10b: The second conductive agent is graphene;

[0135] Embodiment 10c: The second conductive agent is acetylene black.

[0136] Comparative Example 1

[0137] The other conditions of this comparative example group and Example 1 remain unchanged, except that in the preparation of the positive electrode sheet, the conductive agent is all carbon black, the mass ratio of the positive electrode active material, the first conductive agent, the second conductive agent, and the binder is 8:0:1:1, and the coating surface density of the positive electrode sheet is different.

[0138] Comparative Example 1a: Coating surface density is 400g / m 2 ;

[0139] Comparative Example 1b: Coating surface density is 500g / m 2 ;

[0140] Comparative Example 1c: Coating surface density is 600 g / m 2 ;

[0141] Comparative Example 1d: Coating surface density is 700g / m 2 .

[0142] Comparative Example 2

[0143] The other conditions of this comparative example and Example 1 remain unchanged, except that in the preparation of the positive electrode sheet, the conductive agent is all carbon nanotubes, and the mass ratio of the positive electrode active material, the first conductive agent, the second conductive agent, and the binder is 8:0:1:1.

[0144] Comparative Example 3

[0145] The other conditions of this comparative example and Example 6a remain unchanged, except that in the preparation of the positive electrode sheet, the mass ratio of the positive electrode active material, the first conductive agent, the second conductive agent, and the binder is 8:0.2:0.8:1.

[0146] Comparative Example 4

[0147] The other conditions of this comparative example and Example 6a remain unchanged, except that in the preparation of the positive electrode sheet, the coating surface density of the positive electrode sheet is 800 g / m 2 .

[0148] Battery test case

[0149] The lithium-ion batteries of the above embodiments and comparative examples were tested in the following aspects:

[0150] (1) Cracking phenomenon

[0151] When the positive electrode sheet is coated and rolled, the surface cracks of the electrode sheet are visually observed.

[0152] (2) Diaphragm internal resistance

[0153] The positive electrode sheet was punched into discs with a diameter of 50 mm, and the internal resistance of the positive electrode sheet was tested using a resistance meter.

[0154] (3) 25℃ DCR ​​(DC resistance) test

[0155] The experiment was carried out at 25℃, with charge and discharge at 0.5C (current I) for 3 weeks in the range of 2.5-3.65V to fix the capacity, then the charge was adjusted to 50% SOC according to the actual capacity, left to stand for 2h, and then discharged at 1C for 18s. The static cut-off voltage V0 and the 18s discharge cut-off voltage V1 were recorded, and the 25℃ DCR ​​was calculated, DCR=(V0-V1) / I.

[0156] (4) 0.5C rate discharge performance test

[0157] At 25℃, within the charge and discharge cut-off voltage range of 2.5-3.65V, after 3 cycles of charge and discharge at 0.5C, it is recorded as C0. Then it is discharged at 0.5C to 2.5V, recorded as C1. C1 / C0 is the 0.5C rate discharge performance.

[0158] (5) 500-cycle performance test

[0159] Under 25℃ environment, the charge and discharge voltage range is 2.5~3.65V. After the first 3 cycles of 0.5C constant capacity, it is recorded as C0, and the 0.5C charge and discharge cycle begins until C n / C0<80% stops the cycle.

[0160] Table 1

[0161]

[0162] From the above experimental results, it can be seen that after adding the three-dimensional conductive agent of the present invention, the coating surface density of Examples 1 to 10 is 500g / m 2 When the above conditions are met, the charge transfer dynamics of the thick electrode can be improved, the cracking of the positive electrode sheet can be effectively avoided, and the processing performance of the thick electrode sheet can be improved.

[0163] Compared with Example 6a and Examples 8a~c, since the three-dimensional conductive agent of the present invention is not added in Comparative Example 1, the conductive agent is all carbon black, and the carbon black is a one-dimensional particle, it is difficult to form a long-range conductive network, the charge transfer kinetics performance is poor, and as the coating surface density increases, the active material layer of the positive electrode sheet gradually cracks.

[0164] Compared with Example 10a, since Comparative Example 2 does not add the three-dimensional conductive agent of the present invention, the conductive agent is entirely carbon nanotubes. Carbon nanotubes are one-dimensional long tubes, which are difficult to form a three-dimensional conductive network in space. The charge transfer kinetics performance is poor. In addition, due to the lack of spatial stabilization of the three-dimensional conductive agent, the active material layer of the thick electrode plate cracks, affecting the processing performance.

[0165] It can be seen that traditional conductive agents such as carbon black and carbon nanotubes are difficult to form long-range ordered three-dimensional conductive networks in thick electrodes due to their one-dimensional characteristics, resulting in poor charge transfer dynamics. Moreover, due to the lack of spatial stability of the three-dimensional structure of the three-dimensional conductive agent, the cracking phenomenon of the coating becomes more serious as the surface density increases.

[0166] In Comparative Example 3, due to the small amount of three-dimensional conductive agent added in the active material layer, a small amount of cracks appeared in the active material layer of the positive electrode sheet of the thick electrode sheet.

[0167] Comparative Example 4, since the coating surface density is 800g / m 2 The coating surface density is too large, resulting in a large number of cracks in the active material layer of the positive electrode sheet of the thick electrode sheet.

[0168] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a three-dimensional conductive agent, characterized in that: The steps include: Dissolving nanocellulose and metal salt in water, filtering out solids after first ultrasonic stirring, and then drying to obtain powder; In an inert atmosphere, the powder is carbonized to obtain carbon nanowires loaded with metal elements; The carbon nanowires loaded with metal elements and the silane coupling agent are dissolved in an organic solvent, and after a second ultrasonic stirring, a three-dimensional conductive agent is obtained; The three-dimensional conductive agent includes a carbon nanonet having a three-dimensional cross-linked network structure, and the carbon nanonet is a carbon nanonet formed by cross-linking carbon nanowires loaded with metal elements through a silane coupling agent.

2. The method for preparing a three-dimensional conductive agent according to claim 1, characterized in that: The silane coupling agent includes at least one of vinyltrimethoxysilane, vinyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, phenyltrimethoxysilane, γ-aminopropyltrimethoxysilane, 3-glycidyloxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, N-β-aminoethyl-γ-aminopropyltriethoxysilane, methoxytriethylene glycol ether propyltrimethoxysilane, 11-mercaptoundecyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, and diethylphosphoethyltriethoxysilane.

3. The method for preparing a three-dimensional conductive agent according to claim 1 or 2, characterized in that: The metal element includes at least one of aluminum (Al), silver (Ag), and gold (Au).

4. The method for preparing a three-dimensional conductive agent according to claim 1, characterized in that: The mass percentage of the metal salt to the nanocellulose is 5% to 15%.

5. The method for preparing a three-dimensional conductive agent according to claim 1, characterized in that: The mass percentage of the silane coupling agent and the carbon nanowire loaded with metal element is 1% to 3%.

6. The method for preparing a three-dimensional conductive agent according to claim 1, characterized in that: The time of the first ultrasonic stirring or the second ultrasonic stirring is 10 to 30 minutes, and the frequency is 1.6 to 1.8 KHz; And / or, the carbonization temperature is 1100-1300° C., and the time is 4-6 hours.

7. A positive electrode sheet, characterized in that: The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material, a conductive agent and a binder; The conductive agent includes a first conductive agent, or includes a first conductive agent and a second conductive agent; The first conductive agent is the three-dimensional conductive agent prepared by the preparation method according to any one of claims 1 to 6; The second conductive agent includes at least one of carbon black, carbon nanotubes, graphene, and acetylene black.

8. The positive electrode sheet according to claim 7, characterized in that: The coating surface density of the positive electrode active material layer is 400 to 700 g / m 2 .

9. The positive electrode sheet according to claim 7 or 8, characterized in that: The mass percentage of the first conductive agent to the total mass of the conductive agent is 30% to 100%.

10. An electrochemical device, characterized in that: The electrochemical device comprises the positive electrode sheet according to any one of claims 7 to 9.

Citation Information

Patent Citations

  • Thermoplastic resin composition with EMI shielding properties and EMI shielding product prepared thereby

    CN102120891A

  • Method for constructing three-dimensional conductive network in sodium-chloride battery positive pole

    CN104282874A

  • Platinum-based catalyst having high catalytic activity and high durability and adopting porous carbon nano fiber as carrier and preparation method of platinum-based catalyst

    CN104752736A

  • Metallic tin and carbon nanotube co-doped lithium-sulfur battery intermediate layer material and preparation method and application

    CN111900390A

  • Carbon fiber composite material and its forming products, carbon fiber-metal composite material and its forming products, and method of producing the same

    CN1575964A