Energy storage battery connector and preparation method thereof

By using a combination of aluminum-based composite materials and nanomaterials in energy storage battery connectors, the problem of insufficient conductivity and chemical stability in the prior art is solved, and efficient electrical connection and mechanical stability in high temperature and harsh environments are achieved reduces maintenance costs.

CN118263626BActive Publication Date: 2024-11-05SHENZHEN PENGDA INTELLIGENT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410561610.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-08
Publication Date
2024-11-05
Estimated Expiration
2044-05-08

AI Technical Summary

Technical Problem

Existing energy storage battery connectors exhibit weakened conductivity, reduced mechanical strength and insufficient chemical stability in high temperature or harsh environments, resulting in performance degradation and increased maintenance costs.

Method used

Aluminum-based composite material is used as the matrix, combining the composite reinforced materials of gallium nitride nanowires, graphene quantum dots, bismuth telluride nanosheets, molybdenum disulfide nanolayers and perfluorosulfonic acid polymers, and through mechanical mixing and liquid phase peeling , ultrasonic assisted high-energy ball milling, atomic layer deposition and laser sintering, etc., form connectors with excellent conductivity, mechanical strength and chemical stability.

Benefits of technology

It significantly improves the electrical conductivity, mechanical strength and chemical stability of the connector, reduces energy loss and maintenance costs, and is suitable for long-term and high-frequency use in high-temperature and harsh environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a connector for energy storage batteries and a preparation method thereof, wherein the connector structure comprises a base material and a reinforcing filler. The base material adopts an aluminum-based composite material to achieve good mechanical support and conductivity. The reinforcing filler is a composite reinforcing material composed of gallium nitride (GaN) nanowires, graphene quantum dots, bismuth telluride (Bi2Te3) nanosheets, molybdenum disulfide (MoS2) nanolayers and perfluorosulfonic acid polymers (PFSA). These materials each account for 1% to 3% of the base material by weight, and work together to enhance the overall performance of the connector. The present invention not only improves the conductivity and thermal stability of the connector, but also improves the chemical stability and mechanical strength through a unique material combination, and is suitable for various high-performance energy storage systems, especially in applications requiring high reliability and long-term durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of energy storage batteries, and in particular to an energy storage battery connector and a preparation method thereof. Background Art

[0002] In the field of energy storage batteries, connectors are one of the key components. They not only need to provide electrical connections, but also must have excellent mechanical properties, conductivity, and chemical and thermal stability. Battery connectors in existing technologies usually use copper or aluminum as the base material due to their good conductivity and low cost. However, these traditional materials often face the problem of performance degradation under high temperature or harsh environments, such as reduced conductivity and reduced mechanical strength. In order to improve performance, some technologies use composite material technology to combine metal substrates with other metal or non-metal materials to improve the overall performance of the connector.

[0003] Although the existing technology has made some progress, there are still some problems that cannot be ignored. First, while the existing composite connectors improve the conductivity, they often cannot effectively improve the thermal stability and chemical stability, which limits their application in high temperature or chemically corrosive environments. Secondly, the preparation process of traditional composite materials is often complicated and costly, which increases the difficulty of their large-scale production and application. In addition, these materials may age or degrade in performance during long-term use and need to be replaced, thereby increasing maintenance costs.

[0004] Therefore, there is an urgent need to develop a new type of energy storage battery connector. Summary of the invention

[0005] The present application provides an energy storage battery connector and a preparation method thereof, so as to improve the conductivity and thermal stability of the energy storage battery connector.

[0006] The present application provides an energy storage battery connector, comprising a base material and a reinforcing filler; the base material is an aluminum-based composite material;

[0007] The aluminum-based composite material comprises aluminum accounting for 80% by weight of the aluminum-based composite material, graphyne accounting for 10% by weight of the aluminum-based composite material, and silicon carbon nanotubes accounting for 10% by weight of the aluminum-based composite material;

[0008] The reinforcing filler is a composite reinforcing material including gallium nitride GaN nanowires, graphene quantum dots, bismuth telluride Bi2Te3 nanosheets, molybdenum disulfide MoS2 nanolayers and perfluorosulfonic acid polymers, wherein each material in the composite reinforcing material accounts for 1% to 3% of the matrix material by weight.

[0009] Furthermore, the diameter of the gallium nitride nanowire is in the range of 10 nanometers to 100 nanometers, and the length is at least ten times its diameter;

[0010] Furthermore, the average diameter of the graphene quantum dots is less than 10 nanometers.

[0011] Furthermore, the thickness of the bismuth telluride nanosheets is between 5 nanometers and 50 nanometers.

[0012] Furthermore, the number of layers of the molybdenum disulfide nanolayer is 1 to 5; and the molecular weight of the perfluorosulfonic acid polymer is between 100,000 and 500,000 g / mol.

[0013] The present application provides a method for preparing an energy storage battery connector, comprising the following steps:

[0014] (a) providing aluminum powder, graphyne and silicon carbon nanotubes, mixing them in a ratio of 80% aluminum powder, 10% graphyne and 10% silicon carbon nanotubes, and using a mechanical mixing method to ensure that the graphyne and the silicon carbon nanotubes are uniformly dispersed in the aluminum matrix to obtain an aluminum matrix composite material, and using the obtained aluminum matrix composite material as a matrix material;

[0015] (b) providing the required gallium nitride (GaN) nanowires, graphene quantum dots, bismuth telluride (Bi2Te3) nanosheets, molybdenum disulfide (MoS2) nanolayers and perfluorosulfonic acid polymers, wherein the diameter of the gallium nitride nanowires is 10 to 100 nanometers, and the length is at least ten times the diameter; the average diameter of the graphene quantum dots is less than 10 nanometers; the thickness of the bismuth telluride nanosheets is 5 to 50 nanometers; the number of layers of the molybdenum disulfide nanolayers is 1 to 5; the molecular weight of the perfluorosulfonic acid polymer is between 100,000 and 500,000 g / mol; the gallium nitride (GaN) nanowires, graphene quantum dots, bismuth telluride (Bi2Te3) nanosheets, molybdenum disulfide (MoS2) nanolayers and perfluorosulfonic acid polymers are 1% to 3% by weight of the total weight of the matrix material;

[0016] (c) using liquid phase exfoliation technology to separately disperse graphene quantum dots, bismuth telluride nanosheets, and molybdenum sulfide nanolayers to reduce agglomeration and increase their active surface area;

[0017] (d) blending the graphene quantum dots, bismuth telluride nanosheets and molybdenum sulfide nanolayers processed in step c with gallium nitride nanowires, and using ultrasonic-assisted high-energy ball milling to form a more uniform preliminary composite material;

[0018] (e) uniformly depositing a nano-thin layer of a perfluorosulfonic acid polymer on the surface of the preliminary composite reinforcement material formed in step d by atomic layer deposition technology, ensuring that the surface of each nanoparticle is completely covered to improve the interface bonding and chemical stability of the material, thereby generating a composite reinforcement material;

[0019] (f) mixing the aluminum-based composite material obtained in step a with the composite reinforcement material prepared in step e, and compacting the mixture into a connector of a desired shape by laser sintering technology, thereby controlling the microstructure of the material and reducing thermal stress;

[0020] (g) Plasma treatment is performed on the connector having the desired shape formed in step f to further optimize the surface properties and microstructure of the connector.

[0021] The beneficial technical effects of the present invention are embodied in the following aspects:

[0022] (1) The gallium nitride (GaN) nanowires and graphene quantum dots in the composite reinforcement material both have excellent electron mobility and can significantly improve the overall conductivity of the connector. This combined use can ensure that the battery connector can maintain good electrical connection even under high load and reduce energy loss.

[0023] (2) The introduction of bismuth telluride (Bi2Te3) nanosheets and molybdenum disulfide (MoS2) nanolayers not only enhances the mechanical strength of the connector, but also improves its wear and fatigue resistance. This makes the connector more suitable for long-term and high-frequency use conditions and reduces maintenance costs in long-term operation.

[0024] (3) Energy storage systems operating at high temperatures place higher demands on connector materials. Gallium nitride and bismuth telluride, as excellent thermal conductive materials, help improve thermal management and reduce the risk of performance degradation or damage caused by overheating.

[0025] (4) The addition of perfluorosulfonic acid polymer (PFSA) provides a chemically stable protective film for the connector, enhancing its ability to resist corrosion and chemical reactions. This feature enables the connector to maintain its performance in a variety of harsh environments, including applications under acidic or alkaline conditions. DETAILED DESCRIPTION

[0026] Many specific details are described in the following description to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways than those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present application, so the present application is not limited by the specific implementation disclosed below.

[0027] The first embodiment of the present application provides an energy storage battery connector, comprising a base material and a reinforcing filler; the base material is an aluminum-based composite material;

[0028] The aluminum-based composite material comprises aluminum accounting for 80% by weight of the aluminum-based composite material, graphyne accounting for 10% by weight of the aluminum-based composite material, and silicon carbon nanotubes accounting for 10% by weight of the aluminum-based composite material;

[0029] The reinforcing filler is a composite reinforcing material including gallium nitride GaN nanowires, graphene quantum dots, bismuth telluride Bi2Te3 nanosheets, molybdenum disulfide MoS2 nanolayers and perfluorosulfonic acid polymers, wherein each material in the composite reinforcing material accounts for 1% to 3% of the matrix material by weight;

[0030] The diameter of the gallium nitride nanowire is in the range of 10 nanometers to 100 nanometers, and the length is at least ten times its diameter; the average diameter of the graphene quantum dots is less than 10 nanometers; the thickness of the bismuth telluride nanosheet is between 5 nanometers and 50 nanometers; the number of layers of the molybdenum disulfide nanolayer is 1 to 5 layers; and the molecular weight of the perfluorosulfonic acid polymer is between 100,000 and 500,000 g / mol.

[0031] This embodiment provides an energy storage battery connector, including a specially formulated aluminum-based composite material as a matrix material, and a composite reinforcing filler containing multiple nanomaterials. This design is intended to improve the overall performance of the connector, especially in terms of electrical conduction, mechanical stability, and resistance to environmental impact.

[0032] First, regarding the matrix material, the aluminum-based composite material used in this embodiment is composed of three parts: 80% of the total weight is aluminum, which provides good electrical conductivity and processing flexibility; the rest are 10% Graphene and 10% silicon carbon nanotubes. Graphene is a new type of two-dimensional carbon material with excellent mechanical strength and thermal stability, while silicon carbon nanotubes are selected for their high strength and chemical stability. The addition of these two materials significantly enhances the mechanical properties and corrosion resistance of the aluminum-based composite material, while maintaining or improving the electrical conductivity of the material.

[0033] When preparing this aluminum-based composite material, aluminum powder, graphyne and silicon carbon nanotubes are mixed in appropriate proportions. During the mixing process, high-energy ball milling technology is used to ensure that all components are evenly distributed. Subsequently, the matrix material is formed into the desired shape through traditional metal processing techniques such as hot pressing or extrusion molding.

[0034] Secondly, the design of the reinforcing filler includes a variety of different nanoscale materials, each of which is selected based on its unique physical and chemical properties and each accounts for 1% to 3% of the weight of the matrix material. These materials include gallium nitride (GaN) nanowires, graphene quantum dots, bismuth telluride (Bi2Te3) nanosheets, molybdenum disulfide (MoS2) nanolayers, and perfluorosulfonic acid polymers. GaN nanowires provide excellent electron mobility and are suitable for improving conductivity; graphene quantum dots can enhance the density and uniformity of electronic contacts due to their ultra-high surface activity; bismuth telluride nanosheets are selected for their excellent thermoelectric properties, which helps the application of battery connectors in thermoelectric conversion; molybdenum disulfide nanolayers provide good mechanical strength and chemical stability; perfluorosulfonic acid polymers are used as a protective layer to improve the chemical stability and durability of the entire connector.

[0035] When preparing this composite reinforced filler, various nanomaterials are first treated separately by liquid phase exfoliation or ultrasonic dispersion technology to ensure that their active surface area is maximized and agglomeration is reduced. Then, these well-dispersed nanomaterials are thoroughly mixed by high-energy mixing technology, and then combined with atomic layer deposition technology to uniformly deposit perfluorosulfonic acid polymers, thereby forming a uniform and stable composite reinforced filler.

[0036] Finally, the prepared composite reinforced filler is mixed with aluminum-based composite materials, precisely formed by laser sintering or similar technology, and its surface properties and microstructure are further optimized by plasma treatment technology to ensure that the manufactured energy storage battery connector has excellent comprehensive performance in practical applications.

[0037] A detailed test plan is designed below to evaluate and demonstrate the advantages of the energy storage battery connector provided by this embodiment in terms of key performance indicators.

[0038] The testing program includes:

[0039] 1. Conductivity test:

[0040] Test Purpose: To measure the resistance or conductivity of a connector to evaluate its electrical conductivity.

[0041] Test Method: The resistance of the connector is measured under fixed temperature and humidity conditions using a standard four-point probe measurement technique.

[0042] Comparison parameters: The resistance of the connector of the present invention is compared with the resistance of a common aluminum or copper battery connector.

[0043] 2. Mechanical strength test:

[0044] Test purpose: To evaluate the tensile and compressive strength of connectors.

[0045] Test method: Use a universal material testing machine to perform tensile and compressive tests.

[0046] Comparison parameters: Compare the tensile strength and compressive strength of the connector of the present invention with those of the traditional aluminum-based connector.

[0047] 3. Thermal stability test:

[0048] Test purpose: To evaluate the performance changes of connectors in high temperature environments.

[0049] Test method: The connector is heated in a high temperature furnace for a long time and the changes in its conductive and mechanical properties are measured.

[0050] Comparison parameters: Comparison of performance degradation of the connector of the present invention and the traditional connector after high temperature.

[0051] 4. Chemical stability test:

[0052] Test purpose: To evaluate the corrosion resistance and chemical stability of the connector.

[0053] Test method: Immerse the connector in a challenging chemical environment (such as acidic or alkaline solution) and observe the corrosion after a certain period of time.

[0054] Table 1 below provides performance comparison data of the connector A prepared by this embodiment and common aluminum-based connectors and copper-based connectors on the market.

[0055] Table 1, performance data comparison table:

[0056] Performance Indicators Connector A Common aluminum-based connectors Common copper-based connectors Resistance (mOhm cm) 0.015 0.030 0.017 Tensile strength(MPa) 400 300 200 Compressive strength(MPa) 600 400 300 High temperature performance retention rate (%) 95% 80% 85% Corrosion degree slight medium Heavy

[0057] As can be seen from Table 1, the resistance of the energy storage connector A provided in this embodiment is 15 milliohm cm, which is 50% lower than that of common aluminum-based connectors and about 12% lower than that of common copper-based connectors. This shows that by using graphyne and silicon carbon nanotubes as composite reinforcement materials, the present invention has made significant progress in improving the conductivity and is suitable for high-performance battery systems requiring low resistance.

[0058] The energy storage connector A provided in this embodiment has a tensile strength of 400 MPa, which is significantly higher than the 300 MPa of common aluminum-based connectors and the 200 MPa of common copper-based connectors. The compressive strength is 600 MPa, which is much higher than the other two materials. This result is attributed to the high strength characteristics and good interface bonding ability of graphyne and silicon carbon nanotubes, which provide excellent mechanical support and durability.

[0059] At high temperatures, the performance retention rate of the energy storage connector A provided in this embodiment is as high as 95%, while the retention rates of common aluminum-based and copper-based connectors are 80% and 85% respectively. This advantage reflects the superiority of composite materials in thermal stability and temperature resistance, making the connector more stable and reliable in high temperature environments.

[0060] The corrosion test shows that the energy storage connector A provided in this embodiment only shows slight corrosion, while the common aluminum-based and copper-based connectors show moderate and severe corrosion, respectively. This shows that the addition of perfluorosulfonic acid polymer, Graphene and silicon carbon nanotubes enhances the chemical stability of the connector and its ability to resist harsh environments.

[0061] The second embodiment of the present application provides a method for preparing an energy storage battery connector, comprising the following steps:

[0062] (a) providing aluminum powder, graphyne and silicon carbon nanotubes, mixing them in a ratio of 80% aluminum powder, 10% graphyne and 10% silicon carbon nanotubes, and using a mechanical mixing method to ensure that the graphyne and the silicon carbon nanotubes are uniformly dispersed in the aluminum matrix to obtain an aluminum matrix composite material, and using the obtained aluminum matrix composite material as a matrix material;

[0063] (b) providing the required gallium nitride (GaN) nanowires, graphene quantum dots, bismuth telluride (Bi2Te3) nanosheets, molybdenum disulfide (MoS2) nanolayers and perfluorosulfonic acid polymers, wherein the diameter of the gallium nitride nanowires is 10 to 100 nanometers, and the length is at least ten times the diameter; the average diameter of the graphene quantum dots is less than 10 nanometers; the thickness of the bismuth telluride nanosheets is 5 to 50 nanometers; the number of layers of the molybdenum disulfide nanolayers is 1 to 5; the molecular weight of the perfluorosulfonic acid polymer is between 100,000 and 500,000 g / mol; the gallium nitride (GaN) nanowires, graphene quantum dots, bismuth telluride (Bi2Te3) nanosheets, molybdenum disulfide (MoS2) nanolayers and perfluorosulfonic acid polymers are 1% to 3% by weight of the total weight of the matrix material;

[0064] (c) using liquid phase exfoliation technology to separately disperse graphene quantum dots, bismuth telluride nanosheets, and molybdenum sulfide nanolayers to reduce agglomeration and increase their active surface area;

[0065] (d) blending the graphene quantum dots, bismuth telluride nanosheets and molybdenum sulfide nanolayers processed in step c with gallium nitride nanowires, and using ultrasonic-assisted high-energy ball milling to form a more uniform preliminary composite material;

[0066] (e) uniformly depositing a nano-thin layer of a perfluorosulfonic acid polymer on the surface of the preliminary composite reinforcement material formed in step d by atomic layer deposition technology, ensuring that the surface of each nanoparticle is completely covered to improve the interface bonding and chemical stability of the material, thereby generating a composite reinforcement material;

[0067] (f) mixing the aluminum-based composite material obtained in step a with the composite reinforcement material prepared in step e, and compacting the mixture into a connector of a desired shape by laser sintering technology, thereby controlling the microstructure of the material and reducing thermal stress;

[0068] (g) Plasma treatment is performed on the connector having the desired shape formed in step f to further optimize the surface properties and microstructure of the connector.

[0069] First, in the process of preparing the matrix material, aluminum powder, gypsum and silicon carbon nanotubes need to be mixed in a specific ratio (80% aluminum powder, 10% gypsum, 10% silicon carbon nanotubes). Mechanical mixing methods, such as high-energy ball milling, are used to ensure that gypsum and silicon carbon nanotubes are evenly dispersed in the aluminum matrix to form an aluminum-based composite material. This mixing not only increases the overall uniformity of the material, but also helps to improve the mechanical and thermal properties of the final product.

[0070] Next, for the preparation of reinforcing fillers, various nanomaterials need to be provided first, including gallium nitride GaN nanowires, graphene quantum dots, bismuth telluride Bi2Te3 nanosheets, molybdenum disulfide MoS2 nanolayers and perfluorosulfonic acid polymers. The size and quantitative indicators of these materials need to be precisely controlled, such as the diameter and length of gallium nitride nanowires, the diameter of graphene quantum dots, the thickness of bismuth telluride, the number of layers of molybdenum disulfide and the molecular weight of perfluorosulfonic acid polymers. All these materials are added at a ratio of 1% to 3% of the total weight of the matrix material.

[0071] Graphene quantum dots, bismuth telluride nanosheets and molybdenum disulfide nanolayers were treated by liquid phase exfoliation to reduce their agglomeration and increase their active surface area. After treatment, these materials were blended with gallium nitride nanowires and mixed using ultrasound-assisted high-energy ball milling to form a homogeneous preliminary composite material.

[0072] The following details the liquid phase exfoliation treatment of graphene quantum dots, bismuth telluride nanosheets and molybdenum disulfide nanolayers, as well as the specific operation of mixing using ultrasonic-assisted high-energy ball milling.

[0073] Liquid phase exfoliation technology includes the following steps:

[0074] 1. Prepare solvent and dispersant:

[0075] The selection of suitable solvents and dispersants is crucial for successful liquid phase exfoliation. For graphene quantum dots, water or ethanol can be used as solvents due to their good compatibility with graphene; bismuth telluride nanosheets and molybdenum disulfide nanolayers may require non-polar solvents such as xylene to improve their dispersion.

[0076] 2. Dispersed materials:

[0077] Graphene quantum dots, bismuth telluride nanosheets and molybdenum disulfide nanolayers are added to a selected solvent, respectively. Depending on the required processing volume, 1 to 5 grams of nanomaterials are usually added to 100 milliliters of solvent.

[0078] 3. Ultrasonic treatment:

[0079] Ultrasonic treatment is performed using an ultrasonic bath or probe for about 30 minutes to 1 hour to ensure that the material is fully dispersed and the monolayer or few-layer structure is peeled off. The intensity of the ultrasound and the treatment time need to be optimized according to the type of material and the initial particle size.

[0080] 4.Standing and separation:

[0081] The treated mixture is allowed to stand for a period of time to allow the undispersed large particles to settle, and then the upper layer of the suspension containing the nanosheets is taken for subsequent use.

[0082] Ultrasonic-assisted high-energy ball milling includes the following steps:

[0083] 1. Prepare the ball mill:

[0084] Use a suitable ball mill, such as a planetary ball mill, filled with appropriate milling jars and milling media. Steel balls are commonly used for this type of operation as they provide sufficient impact force to achieve effective mixing and further particle size reduction.

[0085] 2. Loading materials:

[0086] In a ball mill, liquid-phase exfoliated graphene quantum dots, bismuth telluride nanosheets and molybdenum disulfide nanolayers are added to the gallium nitride nanowires in a predetermined ratio. The total amount added should not exceed one-third of the tank capacity to ensure sufficient space for mixing.

[0087] 3. Ball milling parameter setting:

[0088] Set the speed and time of the ball mill. Generally, the ball mill speed can be set at 200 to 400 rpm, and the ball mill time can range from a few hours to 24 hours, depending on the degree of mixing of the materials and the particle size requirements.

[0089] 4. Monitoring and post-processing:

[0090] Periodically check the mixing uniformity and particle size changes during the ball milling process. After the ball milling is completed, remove the mixture and, if necessary, remove larger particles that were not fully mixed by screening or centrifugation.

[0091] To enhance the interface bonding and chemical stability of the composite material, a nano-thin layer of perfluorosulfonic acid polymer will be uniformly deposited on the surface of the treated composite material by atomic layer deposition technology. The key to this step is to ensure that the surface of each nanoparticle is completely covered by the perfluorosulfonic acid polymer.

[0092] The following is a detailed description of the process of uniformly depositing a nano-thin layer of a perfluorosulfonic acid polymer on the surface of the treated composite material using atomic layer deposition (ALD) technology.

[0093] First, prepare the atomic layer deposition equipment and ensure that all components, such as the reactor, gas supply system and temperature control system, are in good working condition. Atomic layer deposition is a sophisticated chemical vapor deposition technology that can achieve precise control of single atomic layers and is suitable for forming a uniform and dense protective layer on the surface of nanomaterials.

[0094] Before you begin, place the processed composite materials on the reactor's sample stage. These composite materials may include graphene quantum dots, bismuth telluride nanosheets, molybdenum disulfide nanolayers, and gallium nitride nanowires that have been liquid-phase exfoliated and ultrasonically assisted ball-milled. Make sure the composite materials are evenly distributed so that each particle is evenly covered.

[0095] Next, set the parameters of atomic layer deposition, such as temperature, pressure, and gas flow rate. The deposition of perfluorosulfonic acid polymers usually needs to be carried out at a lower temperature, about 100°C to 200°C, to prevent damage to heat-sensitive materials. The reaction gas usually includes a precursor containing perfluorosulfonic acid polymers and an appropriate reactant, such as water vapor or oxygen, which are alternately introduced into the reactor for surface chemical reactions.

[0096] In the ALD process, the precursor gas of the perfluorosulfonic acid polymer is first introduced to adsorb onto the surface of the composite material. After that, the gas inside the reactor is briefly evacuated to remove the unreacted precursor and byproducts. Next, a reactant (such as water vapor or oxygen) is introduced to promote the decomposition of the precursor to form a nano-thin layer of the perfluorosulfonic acid polymer. This cycle is repeated many times until the desired film thickness is reached.

[0097] The entire ALD process requires precise control and monitoring to ensure the uniformity and quality of the nano-thin layer. After deposition, the composite material is post-processed, such as heat treatment or UV curing, to further enhance the stability and adhesion of the deposited layer.

[0098] Through this method, the surface of each nanoparticle can be completely covered with perfluorosulfonic acid polymer, which significantly improves the chemical stability and interfacial bonding of the composite material. The implementation of this technology not only improves the performance of the material, but also enhances its durability in extreme environments.

[0099] After that, the prepared aluminum-based composite material is mixed with the composite reinforcement material, and the mixture is compacted into the desired shape of the connector by laser sintering technology. Laser sintering technology allows precise control of the sintering process, optimizes the microstructure of the material, reduces thermal stress, and thus improves the performance of the connector. This step not only involves the precise mixing of materials, but also includes the use of advanced manufacturing technology to ensure that the final product has excellent performance and reliability.

[0100] First, the aluminum-based composite material (containing aluminum, graphyne and silicon carbon nanotubes) is thoroughly mixed with various nanoscale reinforcement materials (including gallium nitride GaN nanowires, graphene quantum dots, bismuth telluride Bi2Te3 nanosheets, molybdenum disulfide MoS2 nanolayers and nanoparticles covered with perfluorosulfonic acid polymers). Ensuring that these ingredients are evenly distributed is critical because it directly affects the overall performance of the connector. Using mechanical stirring or slight vibration can help achieve this, but care needs to be taken to avoid destroying the structure of the nanomaterials.

[0101] The mixed material then needs to be formed and solidified through laser sintering technology. Laser sintering is an advanced manufacturing technology that uses a high-energy laser beam to precisely irradiate material powder, locally heating it to a temperature sufficient to melt, thereby solidifying it into a solid shape. In this process, the power, scanning speed and focus size of the laser can be precisely controlled to adjust the sintering conditions and optimize the microstructure of the connector.

[0102] When performing laser sintering, special attention should be paid to the laser scanning path and overlap, which helps to ensure good fusion of the interface between the materials while reducing internal stress caused by uneven heating. By properly setting laser parameters such as scanning speed and laser power, the heating depth and cooling rate can be effectively controlled, thereby reducing thermal stress during sintering.

[0103] After laser sintering, the connector needs to be cooled slowly in a controlled environment to avoid cracks or other structural defects caused by rapid temperature changes. The cooling process is an indispensable part of the entire manufacturing process and is critical to maintaining the structural integrity and long-term stability of the connector.

[0104] Precise laser sintering technology not only improves material utilization and production efficiency, but also ensures that the manufactured connector has excellent mechanical and electrical properties to meet the needs of high-performance battery applications.

[0105] Finally, the molded connector is subjected to plasma treatment, a step designed to further optimize the surface properties and microstructure of the connector, improving its ability to resist environmental influences and its service life.

[0106] Plasma treatment is performed to optimize the surface properties and microstructure of the connector, further enhancing its resistance to environmental influences and service life. Plasma treatment is a sophisticated surface engineering process that can significantly improve the surface properties of the material, such as increasing hardness, improving corrosion resistance and improving the coefficient of friction. The following are the detailed steps for plasma treatment.

[0107] First, the plasma treatment equipment needs to be prepared, which usually includes a vacuum chamber, a high-frequency power supply, and the necessary gas supply system. The equipment should be thoroughly checked beforehand to ensure that all seals, power connections, and control systems are in good condition to ensure the safety and effectiveness of the treatment process.

[0108] Next, the sintered connector is placed in the processing chamber of the plasma treatment device. The processing chamber is first evacuated to a high vacuum to remove any impurities or residual gases that may affect the treatment effect. Under vacuum, specific gases are introduced through the gas supply system. These gases are selected according to the desired treatment effect. Commonly used gases include argon, nitrogen, oxygen and fluorinated gases, which can help form a hard and chemically stable film on the surface of the connector.

[0109] When the required gas pressure and gas composition are reached inside the processing chamber, a high-frequency power supply is used to excite these gases to generate plasma. The high-energy particles of the plasma will act evenly on the surface of the connector to modify its surface properties. The control parameters of this process, including the power of the power supply, the processing time, and the gas flow rate, all need to be precisely controlled to ensure that the desired processing effect is achieved. Typically, the time for plasma treatment ranges from a few minutes to tens of minutes, depending on the nature of the connector material and the required surface characteristics.

[0110] After the plasma treatment is completed, the connector needs to be allowed to cool naturally to room temperature in a controlled environment to avoid thermal stress problems caused by rapid temperature changes. After cooling, the surface and microstructure of the connector should be inspected to ensure that the treatment has achieved the desired improvement.

[0111] Through these steps, plasma treatment can effectively improve the surface quality of the connector, enhance its resistance to environmental influences and service life. In addition, the treatment can also improve the mechanical strength and wear resistance of the connector, making it more suitable for harsh use environments.

[0112] Although the present application is disclosed as above in the form of a preferred embodiment, it is not intended to limit the present application. Any technical personnel in this field may make possible changes and modifications without departing from the spirit and scope of the present application. Therefore, the scope of protection of the present application shall be based on the scope defined by the claims of the present application.

Claims

1. A method for preparing an energy storage battery connector, characterized in that: The following steps are involved: (a) providing aluminum powder, graphyne and silicon carbon nanotubes, mixing them in a ratio of 80% aluminum powder, 10% graphyne and 10% silicon carbon nanotubes, and using a mechanical mixing method to ensure that the graphyne and the silicon carbon nanotubes are uniformly dispersed in the aluminum matrix to obtain an aluminum matrix composite material, and using the obtained aluminum matrix composite material as a matrix material; (b) providing the required gallium nitride (GaN) nanowires, graphene quantum dots, bismuth telluride (Bi2Te3) nanosheets, molybdenum disulfide (MoS2) nanolayers and perfluorosulfonic acid polymers, wherein the diameter of the gallium nitride nanowires is 10 to 100 nanometers, and the length is at least ten times the diameter; the average diameter of the graphene quantum dots is less than 10 nanometers; the thickness of the bismuth telluride nanosheets is 5 to 50 nanometers; the number of layers of the molybdenum disulfide nanolayers is 1 to 5; the molecular weight of the perfluorosulfonic acid polymer is between 100,000 and 500,000 g / mol; the gallium nitride (GaN) nanowires, graphene quantum dots, bismuth telluride (Bi2Te3) nanosheets, molybdenum disulfide (MoS2) nanolayers and perfluorosulfonic acid polymers are 1% to 3% by weight of the total weight of the matrix material; (c) using liquid phase exfoliation technology to separately disperse graphene quantum dots, bismuth telluride nanosheets, and molybdenum sulfide nanolayers to reduce agglomeration and increase their active surface area; (d) blending the graphene quantum dots, bismuth telluride nanosheets and molybdenum sulfide nanolayers processed in step c with gallium nitride nanowires, and using ultrasonic-assisted high-energy ball milling to form a more uniform preliminary composite material; (e) uniformly depositing a nano-thin layer of perfluorosulfonic acid polymer on the surface of the preliminary composite reinforcement material formed in step d by atomic layer deposition technology, ensuring that the surface of each nanoparticle is completely covered to improve the interface bonding and chemical stability of the material, thereby generating a composite reinforcement material; (f) mixing the aluminum-based composite material obtained in step a with the composite reinforcement material prepared in step e, and compacting the mixture into a connector of a desired shape by laser sintering technology, thereby controlling the microstructure of the material and reducing thermal stress; (g) Plasma treatment is performed on the connector having the desired shape formed in step f to further optimize the surface properties and microstructure of the connector.