Oil seal material for engine crankshaft and preparation method thereof
By modifying expanded polytetrafluoroethylene, reinforced filler, compound nano powder and vulcanizing agent, the problem of insufficient mechanical properties of oil sealing materials is solved, and an oil sealing material for engine crankshaft with excellent temperature resistance is prepared, which meets the requirements of High performance requirements for engine crankshaft seals.
Patent Information
- Application Number
- CN202410559496.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-05-08
AI Technical Summary
The mechanical properties of existing oil sealing materials for automobile transmissions are insufficient, mainly due to the poor compatibility of fillers and rubber, which leads to insufficient mechanical properties during use.
The oil sealing material for engine crankshaft is prepared by using modified expanded polytetrafluoroethylene, reinforced fillers, compound nano powder, carbon black and vulcanizing agents. Through specific mixing and vulcanization processes, the oil sealing material for engine crankshafts is improved to improve its mechanical properties and temperature resistance. performance.
It realizes the good mechanical properties and excellent temperature resistance of the oil seal material for engine crankshafts, ensures its quality and quality, is suitable for engine crankshaft seals, and has a broader market prospect.
Smart Images

Figure BDA0004827170460000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil seal materials, in particular to an oil seal material for an engine crankshaft and a preparation method thereof. Background Art
[0002] Oil seal products include fluid sealing materials and non-fluid sealing materials. The sealing effect is directly related to the quality of the oil seal products, and the quality of the oil seal products directly affects the work and production efficiency of the mechanical equipment itself.
[0003] In the patent document with application number "CN201510048593.3" and titled "An oil seal material for automobile gearbox and its preparation method", it is recorded that "the oil seal material for automobile gearbox is composed of the following components in parts by mass: 70-80 parts of acrylate rubber, 20-30 parts of fluororubber, 5-10 parts of octyltin maleate, 2-3 parts of glass fiber, 3-5 parts of stearic acid, 0.5-0.8 parts of calcium carbonate, 3-5 parts of magnesium dimethacrylate, 3-5 parts of drying oil alkyd resin, 1-2 parts of paraffin, 1-1.5 parts of diethanolamine oleate borate, 1-2 parts of diacetyl peroxide, 0.8-1.2 parts of zinc oxide, 8-10 parts of aluminum oxide, 6-8 parts of white carbon black, 0.8-1.5 parts of antioxidant, and 1-3 parts of sulfur. The present invention also provides a preparation method thereof. The oil seal material for automobile gearbox of the present invention has good sealing, high temperature resistance and oil resistance, and is suitable for automobile gearbox sealing."
[0004] Although the oil seal material manufactured by the above patent document has advantages such as high temperature resistance, the compatibility of the filler (such as glass fiber) used by itself with rubber is not good, resulting in relatively insufficient mechanical properties, which still needs further improvement. Based on this, the present invention provides an oil seal material for an engine crankshaft and a preparation method thereof to solve the above technical problems! Summary of the invention
[0005] The purpose of the present invention is to provide an oil seal material for an engine crankshaft and a preparation method thereof. The oil seal material for an engine crankshaft prepared by the present invention not only has good mechanical properties, but also has excellent temperature resistance, effectively ensuring its quality.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] The first aspect of the present invention provides an oil seal material for an engine crankshaft, which is composed of the following raw materials in parts by weight: 20 to 30 parts of modified expanded polytetrafluoroethylene, 3 to 5 parts of reinforcing filler, 4 to 7 parts of composite nanopowder, 2 to 5 parts of carbon black, 2 to 5 parts of stearic acid and 2 to 5 parts of vulcanizing agent.
[0008] Furthermore, the preparation process of the modified expanded polytetrafluoroethylene is as follows:
[0009] Place expanded polytetrafluoroethylene in the modifier at a solid-liquid ratio of 0.012 to 0.022 g / mL, and mix at 4200 to 5200 r / min for 20 to 30 minutes;
[0010] After the mixing is completed, the obtained mixed material is placed in an internal mixer and treated at 150° C. and 120 to 220 r / min for 40 to 46 minutes. After the material is discharged, it is cooled to room temperature to obtain modified expanded polytetrafluoroethylene.
[0011] Furthermore, the modifier is prepared by mixing vinyl silicone oil and dicumyl peroxide in a mass ratio of 1:0.13 to 0.23.
[0012] Furthermore, the preparation process of the reinforcing filler is as follows:
[0013] Place an appropriate amount of the compounded materials in toluene at a mass ratio of 1:4-6, treat at 150-160°C for 250-260 minutes, filter, wash with toluene and deionized water for 2-4 times, and then dry in a drying oven at 60-70°C to constant weight to obtain a first base material;
[0014] Graphene oxide is placed in 1,4-butylene oxide at a solid-liquid ratio of 0.08-0.14 g / mL, and ultrasonically treated for 20-30 min. The resulting suspension is heated to 55-60° C. under an argon atmosphere, and then 0.4-2.2% of diphenylmethane diisocyanate by mass of graphene oxide and 0.02-0.12% of dibutyltin dilaurate by mass of graphene oxide are added, and the mixture is treated at 55-60° C. and 80-90 r / min for 120-140 min. After filtration, the mixture is washed with deionized water for 2-4 times, and then dried in a drying oven at 60-70° C. to constant weight to obtain a second base material;
[0015] The first base material, the second base material, caprolactam and hexamethylene-1,6-diisocyanate are fully mixed in a mass ratio of 1:0.4-0.6:0.1-0.3, and then treated at 170-175°C for 100-200 min.
[0016] The product was washed 2 to 4 times with deionized water and then dried in a drying oven at 60 to 70°C to constant weight to obtain a reinforcing filler.
[0017] Furthermore, the composite material is prepared by mixing halloysite nanotubes, diphenylmethane diisocyanate and dibutyltin dilaurate in a mass ratio of 1:2.2-2.4:0.01-0.03.
[0018] Furthermore, the compound nano powder is compounded by nano titanium dioxide and nano zinc oxide in a mass ratio of 1:0.2-0.4.
[0019] Furthermore, the antioxidant is selected from any one of antioxidant 1010, antioxidant 1076, and antioxidant CA.
[0020] Furthermore, the vulcanizing agent is selected from any one of dicumyl peroxide and benzoyl peroxide.
[0021] The second aspect of the present invention: also provides a method for preparing the above-mentioned engine crankshaft oil seal material, comprising the following steps:
[0022] Step 1, accurately weighing modified expanded polytetrafluoroethylene, reinforcing filler, compound nano powder, carbon black, stearic acid and vulcanizing agent, and putting the modified expanded polytetrafluoroethylene, reinforcing filler, compound nano powder, carbon black, stearic acid and vulcanizing agent into a mixing device for mixing and stirring, and then placing them in a microwave device and treating them for 10 to 12 minutes under the condition of a microwave power of 320 to 340 w, and finally transferring the obtained materials into a mixer and performing an open refining process at a temperature of 150 to 160 ° C;
[0023] Step 2: Then the mixed rubber obtained by the open mill is subjected to a second-stage vulcanization to obtain a finished product of an oil seal material for an engine crankshaft.
[0024] Furthermore, in the step 2, the process of the two-stage vulcanization is as follows:
[0025] The first stage of vulcanization: the vulcanization temperature is 150-170°C, the vulcanization time is 30-40 minutes, and the vulcanization pressure is 9-12MPa;
[0026] Second stage vulcanization: Carry out the second stage vulcanization in an oven at 150-170°C for 60-70 minutes.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] In the present invention, modified expanded polytetrafluoroethylene, reinforcing filler, compounded nano powder, carbon black, stearic acid and vulcanizing agent are used as raw materials, and the modified expanded polytetrafluoroethylene, reinforcing filler, compounded nano powder, carbon black, stearic acid and vulcanizing agent are accurately weighed, and the modified expanded polytetrafluoroethylene, reinforcing filler, compounded nano powder, carbon black, stearic acid and vulcanizing agent are put into a mixing device for mixing and stirring, and then placed in a microwave device for processing. Finally, the obtained material is transferred to a mixer for refining processing, and then the refining rubber obtained by refining is vulcanized in two stages to obtain a finished product of an engine crankshaft oil seal material. The engine crankshaft oil seal material prepared by the present invention not only has good mechanical properties, but also has excellent temperature resistance, which effectively guarantees its quality and quality. The engine crankshaft oil seal material and preparation method thereof provided by the present invention have a broader market prospect and are more suitable for promotion. DETAILED DESCRIPTION
[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Example 1
[0031] The present embodiment provides an oil seal material for an engine crankshaft, which is composed of the following raw materials in parts by weight: 20 parts of modified expanded polytetrafluoroethylene, 3 parts of reinforcing filler, 4 parts of compound nano powder, 2 parts of carbon black, 2 parts of stearic acid and 2 parts of vulcanizing agent.
[0032] Among them, the preparation process of modified expanded polytetrafluoroethylene is as follows:
[0033] Expanded polytetrafluoroethylene was placed in the modifier at a solid-liquid ratio of 0.012 g / mL and mixed at 4200 r / min for 20 min;
[0034] After the mixing is completed, the obtained mixture is placed in an internal mixer and treated at 150° C. and 120 r / min for 40 min. After being discharged, the mixture is cooled to room temperature to obtain modified expanded polytetrafluoroethylene.
[0035] Furthermore, the modifier is prepared by mixing vinyl silicone oil and dicumyl peroxide in a mass ratio of 1:0.13.
[0036] In this embodiment, it should be noted that expanded polytetrafluoroethylene was purchased from Hejian Fenghang Sealing Material Co., Ltd., and vinyl silicone oil was purchased from Jinan Xinglongda Chemical Co., Ltd.
[0037] In addition, the preparation process of the reinforcing filler is as follows:
[0038] Place an appropriate amount of the compounded materials in toluene at a mass ratio of 1:4, treat at 150°C for 250 minutes, filter, wash twice with toluene and deionized water, respectively, and then dry in a drying oven at 60°C to constant weight to obtain a first base material;
[0039] Graphene oxide was placed in 1,4-butylene oxide at a solid-liquid ratio of 0.08 g / mL, and ultrasonically treated for 20 min. The resulting suspension was heated to 55° C. under an argon atmosphere, and then 0.4% of diphenylmethane diisocyanate and 0.02% of dibutyltin dilaurate were added to the suspension, and the suspension was treated at 55° C. and 80 r / min for 120 min. After filtration, the suspension was washed with deionized water twice, and then dried in a drying oven at 60° C. to constant weight to obtain a second base material.
[0040] The first base material, the second base material, caprolactam and hexamethylene-1,6-diisocyanate were fully mixed in a mass ratio of 1:0.4:0.1, and then treated at 170°C for 100 minutes. The obtained product was washed twice with deionized water and then dried in a drying oven at 60°C to constant weight to obtain a reinforcing filler.
[0041] Furthermore, the composite material is prepared by mixing halloysite nanotubes, diphenylmethane diisocyanate and dibutyltin dilaurate in a mass ratio of 1:2.2:0.01.
[0042] In this embodiment, it should be noted that the halloysite nanotubes were purchased from Suzhou Kaifa New Material Technology Co., Ltd., and the graphene oxide was purchased from Suzhou Beike Nanotechnology Co., Ltd.
[0043] In addition, the compound nano powder is compounded by nano titanium dioxide and nano zinc oxide in a mass ratio of 1:0.2.
[0044] In addition, antioxidant 1010 is selected as the antioxidant.
[0045] The vulcanizing agent is diisopropylbenzene peroxide.
[0046] In addition, this embodiment also provides a method for preparing the above-mentioned engine crankshaft oil seal material, comprising the following steps:
[0047] Step 1, accurately weighing modified expanded polytetrafluoroethylene, reinforcing filler, compound nano powder, carbon black, stearic acid and vulcanizing agent, and putting the modified expanded polytetrafluoroethylene, reinforcing filler, compound nano powder, carbon black, stearic acid and vulcanizing agent into a mixing device for mixing and stirring, and then placing them in a microwave device and treating them for 10 minutes under the condition of a microwave power of 320W, and finally transferring the obtained materials into a mixer and performing an open refining process at a temperature of 150°C;
[0048] Step 2: Then the mixed rubber obtained by the open mill is subjected to a second-stage vulcanization to obtain a finished product of an oil seal material for an engine crankshaft.
[0049] Among them, the process of two-stage vulcanization is as follows:
[0050] The first stage of vulcanization: the vulcanization temperature is 150°C, the vulcanization time is 30 minutes, and the vulcanization pressure is 9 MPa;
[0051] Second stage vulcanization: The second stage vulcanization is carried out in an oven at 150°C for 60 minutes.
[0052] Example 2
[0053] The preparation method of the engine crankshaft oil seal material provided in this embodiment is basically the same as that in Example 1, except that: the specific raw material composition and specific preparation method of the engine crankshaft oil seal material in this embodiment are different; the specific raw material composition and specific preparation method of the engine crankshaft oil seal material in this embodiment are as follows:
[0054] An oil seal material for an engine crankshaft is composed of the following raw materials in parts by weight: 25 parts of modified expanded polytetrafluoroethylene, 4 parts of reinforcing fillers, 5 parts of compound nano powders, 3 parts of carbon black, 3 parts of stearic acid and 3 parts of vulcanizing agent.
[0055] Among them, the preparation process of modified expanded polytetrafluoroethylene is as follows:
[0056] Expanded polytetrafluoroethylene was placed in the modifier at a solid-liquid ratio of 0.017 g / mL and mixed at 4700 r / min for 25 min;
[0057] After the mixing is completed, the obtained mixture is placed in an internal mixer and treated at 150° C. and 170 r / min for 43 min. After being discharged, the mixture is cooled to room temperature to obtain modified expanded polytetrafluoroethylene.
[0058] Furthermore, the modifier is prepared by mixing vinyl silicone oil and dicumyl peroxide in a mass ratio of 1:0.18.
[0059] In this embodiment, it should be noted that expanded polytetrafluoroethylene was purchased from Hejian Fenghang Sealing Material Co., Ltd., and vinyl silicone oil was purchased from Jinan Xinglongda Chemical Co., Ltd.
[0060] In addition, the preparation process of the reinforcing filler is as follows:
[0061] Place an appropriate amount of the compounded materials in toluene at a mass ratio of 1:5, treat at 155°C for 255 minutes, filter, wash with toluene and deionized water three times, and then dry in a drying oven at 65°C to constant weight to obtain a first base material;
[0062] Graphene oxide was placed in 1,4-butylene oxide at a solid-liquid ratio of 0.11 g / mL, and ultrasonically treated for 25 minutes. The resulting suspension was heated to 57°C under an argon atmosphere, and then 1.4% of diphenylmethane diisocyanate and 0.07% of dibutyltin dilaurate were added to the suspension. The suspension was treated at 57°C and 85 r / min for 130 minutes. After filtration, the suspension was washed with deionized water for 3 times, and then dried in a drying oven at 65°C to constant weight to obtain a second base material.
[0063] The first base material, the second base material, caprolactam and hexamethylene-1,6-diisocyanate were fully mixed in a mass ratio of 1:0.5:0.2, and then treated at 172°C for 105 minutes. The obtained product was washed three times with deionized water and then dried in a drying oven at 65°C to constant weight to obtain a reinforcing filler.
[0064] Furthermore, the composite material is prepared by mixing halloysite nanotubes, diphenylmethane diisocyanate and dibutyltin dilaurate in a mass ratio of 1:2.3:0.02.
[0065] In this embodiment, it should be noted that the halloysite nanotubes were purchased from Suzhou Kaifa New Material Technology Co., Ltd., and the graphene oxide was purchased from Suzhou Beike Nanotechnology Co., Ltd.
[0066] In addition, the compound nano powder is compounded by nano titanium dioxide and nano zinc oxide in a mass ratio of 1:0.3.
[0067] In addition, antioxidant 1076 is selected as the antioxidant.
[0068] Benzoyl peroxide is used as the vulcanizing agent.
[0069] In addition, this embodiment also provides a method for preparing the above-mentioned engine crankshaft oil seal material, comprising the following steps:
[0070] Step 1, accurately weighing modified expanded polytetrafluoroethylene, reinforcing filler, compounded nano powder, carbon black, stearic acid and vulcanizing agent, and putting the modified expanded polytetrafluoroethylene, reinforcing filler, compounded nano powder, carbon black, stearic acid and vulcanizing agent into a mixing device for mixing and stirring, and then placing them in a microwave device and treating them for 11 minutes under the condition of a microwave power of 330W, and finally transferring the obtained materials into a mixer and performing an open refining process at a temperature of 155°C;
[0071] Step 2: Then the mixed rubber obtained by the open mill is subjected to a second-stage vulcanization to obtain a finished product of an oil seal material for an engine crankshaft.
[0072] Among them, the process of two-stage vulcanization is as follows:
[0073] The first stage of vulcanization: the vulcanization temperature is 160℃, the vulcanization time is 35min, and the vulcanization pressure is 10MPa;
[0074] Second stage vulcanization: The second stage vulcanization is carried out in an oven at 160°C for 65 minutes.
[0075] Example 3
[0076] The preparation method of the engine crankshaft oil seal material provided in this embodiment is basically the same as that in Example 1, except that: the specific raw material composition and specific preparation method of the engine crankshaft oil seal material in this embodiment are different; the specific raw material composition and specific preparation method of the engine crankshaft oil seal material in this embodiment are as follows:
[0077] An oil seal material for an engine crankshaft is composed of the following raw materials in parts by weight: 30 parts of modified expanded polytetrafluoroethylene, 5 parts of reinforcing filler, 7 parts of compound nano powder, 5 parts of carbon black, 5 parts of stearic acid and 5 parts of vulcanizing agent.
[0078] Among them, the preparation process of modified expanded polytetrafluoroethylene is as follows:
[0079] Expanded polytetrafluoroethylene was placed in the modifier at a solid-liquid ratio of 0.022 g / mL and mixed at 5200 r / min for 30 min;
[0080] After the mixing is completed, the obtained mixture is placed in an internal mixer and treated at 150° C. and 220 r / min for 46 min. After being discharged, the mixture is cooled to room temperature to obtain modified expanded polytetrafluoroethylene.
[0081] Furthermore, the modifier is prepared by mixing vinyl silicone oil and diisopropylbenzene peroxide in a mass ratio of 1:0.23.
[0082] In this embodiment, it should be noted that expanded polytetrafluoroethylene was purchased from Hejian Fenghang Sealing Material Co., Ltd., and vinyl silicone oil was purchased from Jinan Xinglongda Chemical Co., Ltd.
[0083] In addition, the preparation process of the reinforcing filler is as follows:
[0084] Place an appropriate amount of the compounded materials in toluene at a mass ratio of 1:6, treat at 160°C for 260 minutes, filter, wash with toluene and deionized water for 4 times, and then dry in a drying oven at 70°C to constant weight to obtain a first base material;
[0085] Graphene oxide was placed in 1,4-butylene oxide at a solid-liquid ratio of 0.14 g / mL, and ultrasonically treated for 30 minutes. The resulting suspension was heated to 60°C under an argon atmosphere, and then 2.2% of diphenylmethane diisocyanate and 0.12% of dibutyltin dilaurate were added to the suspension. The suspension was treated at 60°C and 90 r / min for 140 minutes. After filtration, the suspension was washed with deionized water for 4 times, and then dried in a drying oven at 70°C to constant weight to obtain a second base material.
[0086] The first base material, the second base material, caprolactam and hexamethylene-1,6-diisocyanate were fully mixed in a mass ratio of 1:0.6:0.3, and then treated at 175°C for 110 minutes. The obtained product was washed 4 times with deionized water and then dried in a drying oven at 70°C to constant weight to obtain a reinforcing filler.
[0087] Furthermore, the composite material is prepared by mixing halloysite nanotubes, diphenylmethane diisocyanate and dibutyltin dilaurate in a mass ratio of 1:2.4:0.03.
[0088] In this embodiment, it should be noted that the halloysite nanotubes were purchased from Suzhou Kaifa New Material Technology Co., Ltd., and the graphene oxide was purchased from Suzhou Beike Nanotechnology Co., Ltd.
[0089] In addition, the compound nano powder is compounded by nano titanium dioxide and nano zinc oxide in a mass ratio of 1:0.4.
[0090] In addition, antioxidants are selected.
[0091] The vulcanizing agent is diisopropylbenzene peroxide.
[0092] In addition, this embodiment also provides a method for preparing the above-mentioned engine crankshaft oil seal material, comprising the following steps:
[0093] Step 1, accurately weighing modified expanded polytetrafluoroethylene, reinforcing filler, compound nano powder, carbon black, stearic acid and vulcanizing agent, and putting the modified expanded polytetrafluoroethylene, reinforcing filler, compound nano powder, carbon black, stearic acid and vulcanizing agent into a mixing device for mixing and stirring, and then placing them in a microwave device and treating them for 12 minutes under the condition of a microwave power of 340W, and finally transferring the obtained materials into a mixer and performing an open refining process at a temperature of 160°C;
[0094] Step 2: Then the mixed rubber obtained by the open mill is subjected to a second-stage vulcanization to obtain a finished product of an oil seal material for an engine crankshaft.
[0095] Among them, the process of two-stage vulcanization is as follows:
[0096] The first stage of vulcanization: the vulcanization temperature is 170℃, the vulcanization time is 40min, and the vulcanization pressure is 12MPa;
[0097] Second stage vulcanization: The second stage vulcanization is carried out in an oven at 170°C for 70 minutes.
[0098] Comparative Example 1: The difference from Example 1 is that in this example, an equal amount of expanded polytetrafluoroethylene is used instead of modified expanded polytetrafluoroethylene.
[0099] Comparative Example 2: The difference from Example 1 is that in this example, an equal amount of graphene oxide is used instead of the reinforcing filler.
[0100] Comparative Example 3: The difference from Example 1 is that in this example, microwave treatment is not performed in step 1.
[0101] Performance test: The samples of the engine crankshaft oil seal materials provided in Examples 1 to 3 and Comparative Examples 1 to 3 are marked as Examples 1 to 3 and Comparative Examples 1 to 3, respectively; and the relevant properties of the engine crankshaft oil seal materials provided in Examples 1 to 3 and Comparative Examples 1 to 3 are tested as follows:
[0102] 1. Abrasion test: The test method is GB / T3960-1983.
[0103] 2. Friction coefficient test: The test method is GB / T3960-1983.
[0104] 3. Tensile test: The test method is HGT2902-1997.
[0105] 4. Elongation at break test: The test method is HGT2902-1997.
[0106] 5. Temperature resistance test: Place in a high temperature box at 150℃*70h, then take it out, cool it to room temperature, and perform a tensile test using a tensile testing machine. If the tensile strength of the product is ≥10MPa and the elongation is ≥150%, the high temperature resistance performance is recorded as "qualified"; if the tensile strength of the product is <10MPa or the elongation is <150%, the high temperature resistance performance is recorded as "unqualified".
[0107] The obtained test data are recorded in Table 1 and Table 2 below:
[0108] Table 1 Mechanical properties test results of each group of oil seal materials
[0109]
[0110]
[0111] Table 2 Test results of temperature resistance of oil seal materials in each group
[0112] Group Heat resistance effect Example 1 Group qualified Example 2 Group qualified Example 3 Group qualified Comparison group 1 Failure Comparison of 2 groups Failure Comparison of 3 groups Failure
[0113] By comparing and analyzing the relevant data in Table 1 and Table 2, it can be seen that the engine crankshaft oil seal material prepared by the present invention not only has good mechanical properties, but also has excellent temperature resistance, effectively ensuring its quality. This shows that the engine crankshaft oil seal material and the preparation method thereof provided by the present invention have a broader market prospect and are more suitable for promotion.
[0114] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0115] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. An oil seal material for an engine crankshaft, characterized in that: The invention is composed of the following raw materials in parts by weight: 20 to 30 parts of modified expanded polytetrafluoroethylene, 3 to 5 parts of reinforcing fillers, 4 to 7 parts of compound nano powders, 2 to 5 parts of carbon black, 2 to 5 parts of stearic acid and 2 to 5 parts of vulcanizing agent; The preparation process of the modified expanded polytetrafluoroethylene is as follows: Place expanded polytetrafluoroethylene in the modifier at a solid-liquid ratio of 0.012 to 0.022 g / mL, and mix at 4200 to 5200 r / min for 20 to 30 minutes; After the mixing is completed, the obtained mixed material is placed in an internal mixer, and processed at 150° C. and 120 to 220 r / min for 40 to 46 minutes, and then cooled to room temperature after being discharged to obtain modified expanded polytetrafluoroethylene; The modifier is prepared by mixing vinyl silicone oil and dicumyl peroxide in a mass ratio of 1:0.13 to 0.23; The preparation process of the reinforcing filler is as follows: Place an appropriate amount of the compounded materials in toluene at a mass ratio of 1:4-6, treat at 150-160°C for 250-260 minutes, filter, wash with toluene and deionized water for 2-4 times, and then dry in a drying oven at 60-70°C to constant weight to obtain a first base material; Graphene oxide is placed in 1,4-butylene oxide at a solid-liquid ratio of 0.08-0.14 g / mL, and ultrasonically treated for 20-30 min. The resulting suspension is heated to 55-60° C. under an argon atmosphere, and then 0.4-2.2% of diphenylmethane diisocyanate and 0.02-0.12% of dibutyltin dilaurate are added. The mixture is treated at 55-60° C. and 80-90 r / min for 120-140 min. After filtration, the mixture is washed with deionized water for 2-4 times, and then dried in a drying oven at 60-70° C. to constant weight to obtain a second base material. The first base material, the second base material, caprolactam and hexamethylene-1,6-diisocyanate are fully mixed in a mass ratio of 1:0.4-0.6:0.1-0.3, and then treated at 170-175° C. for 100-110 min. The obtained product is washed with deionized water for 2-4 times, and then dried in a drying oven at 60-70° C. to constant weight to obtain a reinforcing filler; The composite material is prepared by mixing halloysite nanotubes, diphenylmethane diisocyanate and dibutyltin dilaurate in a mass ratio of 1:2.2-2.4:0.01-0.03; The method for preparing the oil seal material for the engine crankshaft comprises the following steps: Step 1, accurately weighing modified expanded polytetrafluoroethylene, reinforcing filler, compound nano powder, carbon black, stearic acid and vulcanizing agent, and putting the modified expanded polytetrafluoroethylene, reinforcing filler, compound nano powder, carbon black, stearic acid and vulcanizing agent into a mixing device for mixing and stirring, and then placing them in a microwave device and treating them for 10 to 12 minutes under the condition of a microwave power of 320 to 340 w, and finally transferring the obtained materials into a mixer and performing an open refining process at a temperature of 150 to 160 ° C; Step 2: Then the mixed rubber obtained by the open mill is subjected to a second-stage vulcanization to obtain a finished product of an oil seal material for an engine crankshaft.
2. The oil seal material for an engine crankshaft according to claim 1, characterized in that: The compound nano powder is compounded by nano titanium dioxide and nano zinc oxide in a mass ratio of 1:0.2-0.
4.
3. The oil seal material for an engine crankshaft according to claim 1, characterized in that: The antioxidant is selected from any one of antioxidant 1010, antioxidant 1076, and antioxidant CA.
4. The oil seal material for an engine crankshaft according to claim 1, characterized in that: The vulcanizing agent is selected from any one of dicumyl peroxide and benzoyl peroxide.
5. The method for preparing an oil seal material for an engine crankshaft according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1, accurately weighing modified expanded polytetrafluoroethylene, reinforcing filler, compound nano powder, carbon black, stearic acid and vulcanizing agent, and putting the modified expanded polytetrafluoroethylene, reinforcing filler, compound nano powder, carbon black, stearic acid and vulcanizing agent into a mixing device for mixing and stirring, and then placing them in a microwave device and treating them for 10 to 12 minutes under the condition of a microwave power of 320 to 340 w, and finally transferring the obtained materials into a mixer and performing an open refining process at a temperature of 150 to 160 ° C; Step 2: Then the mixed rubber obtained by the open mill is subjected to a second-stage vulcanization to obtain a finished product of an oil seal material for an engine crankshaft.
6. The method for preparing an oil seal material for an engine crankshaft according to claim 5, characterized in that: In the step 2, the process of the two-stage vulcanization is as follows: The first stage of vulcanization: the vulcanization temperature is 150-170°C, the vulcanization time is 30-40 minutes, and the vulcanization pressure is 9-12 MPa; Second stage vulcanization: The second stage vulcanization is carried out in an oven at 150-170°C for 60-70 minutes.