A high-toughness, high-durability marine engineering concrete protective coating and preparation method thereof
Through the combination of anionic water-based polyurethane and fast hard and early strength cement, a high toughness and high durability protective coating of offshore concrete is formed, which solves the problem of easy erosion of offshore concrete in seawater environment and achieves high adhesion of the coating. Resistance to seepage and ductility, suitable for repair protection in marine engineering.
Patent Information
- Application Number
- CN202410327740.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-21
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-03-21
AI Technical Summary
Offshore concrete is easily eroded by chloride ions and sulfate ions in seawater environments, resulting in reduced durability. Traditional protective coatings have problems such as low toughness, poor adhesion and insufficient permeability.
Anionic water-based polyurethane is combined with fast hard and early-strength cement, and the macromolecular network structure is formed through electrostatic adsorption and complexation reaction, which enhances the crack resistance and ductility of the coating, and forms a solid form through the hydrolysis reaction of silicone contact with water. Si-O-Si bonds improve bonding strength, while using early-strength, low-carbon sulfur aluminate cement and homemade anionic aqueous polyurethane emulsions to improve the compatibility and durability of the coating.
It significantly improves the crack resistance, ductility and bonding strength of the coating, enhances its resistance to harmful ions and water, extends the service life of concrete structures, and reduces construction costs.
Smart Images

Figure CN118271883B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of marine engineering concrete protective materials, and in particular to a high-toughness and high-durability marine engineering concrete protective coating and a preparation method thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] At present, concrete engineering construction is gradually expanding to the ocean, but the chloride ions and sulfate ions in seawater will corrode concrete and affect the durability of concrete. Chloride ions can destroy the passivation film of concrete steel bars and accelerate the corrosion of steel bars. Low concentrations of chloride ions react with the cement hydration product polysulfide hydrated calcium sulfoaluminate (AFm) to form Kuzel salt; high concentrations of chloride ions react with AFm to form Friedel salt, reducing the production of hydration products such as ettringite. Sulfate ions react with the hydration product AFm to form secondary ettringite, which doubles in volume and causes expansion damage. Sulfate ions can also react with the hydration product calcium hydroxide to form secondary gypsum, which causes volume expansion damage. Seawater contains both chloride ions and sulfate ions, which work together to corrode concrete more severely than the corrosion under separate conditions. A large number of engineering examples show that under harsh environmental conditions, marine concrete structures will be destroyed within five years and will be unusable within ten years, let alone reach the expected service life of a hundred years. Therefore, how to protect marine concrete has become an urgent problem to be solved in the construction industry.
[0004] Applying protective coatings on the surface of marine concrete can protect marine concrete. Traditional protective coatings are mainly divided into two categories: inorganic coatings and organic coatings. Inorganic coatings are mainly composed of pure cement-based materials and have strong anti-aging and durability. However, they have problems such as low toughness, poor adhesion and low impermeability. Organic coatings are mainly composed of carbon and hydrogen compounds, such as epoxy resin, acrylic acid and styrene-butadiene rubber. These organic coatings have excellent film-forming properties and effectively prevent water and harmful ions from invading the concrete matrix. Nevertheless, the adhesion between organic coatings and inorganic matrices is poor and the impact resistance is weak. In addition, due to the presence of aromatic hydrocarbon groups, many organic materials tend to yellow when exposed to sunlight. Therefore, a new type of protective coating with high adhesion, high toughness and high durability is urgently needed. Summary of the invention
[0005] In order to overcome the above problems, the present invention provides a high-toughness, high-durability marine engineering concrete protective coating and a preparation method thereof.
[0006] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0007] The first aspect of the present invention provides a high-toughness and high-durability marine engineering concrete protective coating, the raw materials of which include, by weight: 95 to 105 parts of fast-hardening and early-strength cement, 0 to 50 parts of anionic water-based polyurethane, 0 to 1 part of defoaming agent, 0.2 to 1 part of water reducing agent, 0.1 to 1 part of early-strength agent, and 5 to 40 parts of mixing water.
[0008] The preparation method of the anionic waterborne polyurethane comprises:
[0009] (1) mixing isophorone diisocyanate and polyethylene glycol uniformly and performing a first heating and stirring reaction;
[0010] (2) adding dimethylolpropionic acid to the reaction system of step (1) and performing a second heating and stirring reaction;
[0011] (3) adding triethylamine to the reaction system of step (2) and performing a third stirring reaction;
[0012] (4) adding N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane to the reaction system of step (3) and performing a fourth stirring reaction;
[0013] (5) Finally, distilled water is added to the reaction system of step (4), and the reaction is stirred for the fifth time to finally obtain anionic waterborne polyurethane.
[0014] The second aspect of the present invention provides a method for preparing the above-mentioned high-toughness and high-durability marine engineering concrete protective coating, comprising:
[0015] Mix the anionic water-based polyurethane and mixing water evenly according to the ratio, then add the fast-hardening and early-strength cement, mix evenly, and add the defoamer, water-reducing agent and early-strength agent during the stirring process.
[0016] The beneficial effects of the present invention are:
[0017] (1) Through electrostatic adsorption and complexation reaction, the hydroxyl and carboxyl groups in the anionic waterborne polyurethane form a metal cation Ca in the cement matrix. 2+ and Al 3+The network is a macromolecular network structure with sulfoaluminate cement as the center. The network is a bridge connecting the polymer film and cement hydration products. In addition, during the hydration of sulfoaluminate cement, the rapid consumption of water and the release of high heat enhance the film-forming effect of the anionic waterborne polyurethane, resulting in mutual penetration between the anionic waterborne polyurethane and the cement hydration products, forming a continuous phase composite interpenetrating network structure, thereby improving the crack resistance and ductility of the coating. In addition, due to the hydrolysis reaction of siloxane on the surface of the anionic waterborne polyurethane in contact with water, silanol and volatile methanol are produced. A part of the silanol further undergoes a condensation reaction with the hydroxyl group on the surface of calcium hydroxide in the concrete matrix to form a strong Si-O-Si bond, which enhances the bonding strength. At the same time, the presence of a large nucleation zone in the anionic waterborne polyurethane promotes the precipitation of substances such as CSH gel at the interface between the polymer film and cement paste, further improving the bonding strength.
[0018] (2) Compared with the prior art, the sulphoaluminate cement used in the present invention has the characteristics of early strength, low carbon, low shrinkage, and acid and alkali resistance. The homemade anionic water-based polyurethane emulsion has the characteristics of high flexibility, high adhesion, solubility in water, and no volatility. The two have good compatibility after mixing, which improves the working performance of the coating. A multi-phase composite continuous interpenetrating network structure is formed inside the system, which improves the ductility and bonding strength of the coating, while reducing the corrosion of external harmful ions and aqueous solutions, and effectively improves the durability and impermeability of the repair protective coating. In addition, the reduction of pores inside the system reduces the cracking of the coating and ensures the volume stability of the coating. The repair protective coating of the present invention has a wide range of applications, is less affected by the environment during construction, has a simple construction process, and does not require additional maintenance measures after the construction is completed, which greatly reduces the construction cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0020] Figure 1 The 7-day tensile strength test results of the marine concrete protective coatings of Examples 1 to 3 and Comparative Examples 1 to 4;
[0021] Figure 2 The 7-day bonding strength test results of the marine concrete protective coatings of Examples 1 to 3 and Comparative Examples 1 to 4;
[0022] Figure 3 The carbonization depth test results of 28 hours after the concrete substrate was coated with the marine concrete protective coatings of Examples 1 to 3 and Comparative Examples 1 to 4;
[0023] Figure 4The results of the anti-permeability test of the mortar substrate after coating the marine concrete protective coatings of Examples 1 to 3 and Comparative Examples 1 to 4;
[0024] Figure 5 These are the test results of the sulfuric acid corrosion resistance of the mortar substrate after coating the marine concrete protective coatings of Examples 1 to 3 and Comparative Examples 1 to 4. DETAILED DESCRIPTION
[0025] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0026] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0027] The first typical embodiment of the present invention provides a high-toughness and high-durability marine engineering concrete protective coating, the raw materials of which include, by weight: 95 to 105 parts of fast-hardening and early-strength cement, 0 to 50 parts of anionic water-based polyurethane, 0 to 1 part of defoaming agent, 0.2 to 1 part of water reducing agent, 0.1 to 1 part of early strength agent, and 5 to 40 parts of mixing water.
[0028] In one or more embodiments, the method for preparing the anionic waterborne polyurethane comprises:
[0029] (1) mixing isophorone diisocyanate and polyethylene glycol uniformly and performing a first heating and stirring reaction;
[0030] (2) adding dimethylolpropionic acid to the reaction system of step (1) and performing a second heating and stirring reaction;
[0031] (3) adding triethylamine to the reaction system of step (2) and performing a third stirring reaction;
[0032] (4) adding N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane to the reaction system of step (3) and performing a fourth stirring reaction;
[0033] (5) Finally, distilled water is added to the reaction system of step (4), and the reaction is stirred for the fifth time to finally obtain anionic waterborne polyurethane.
[0034] The reaction process of anionic waterborne polyurethane includes: diisocyanate reacts with polyethylene glycol to generate the most basic functional group of waterborne polyurethane - carbamate. Isophorone diisocyanate is selected here because it has excellent hydrolysis resistance and aging resistance. Dimethylol propionic acid is the best hydrophilic chain extender for preparing ionic anionic waterborne polyurethane. Its neopentyl glycol structure improves the heat resistance and hydrolysis resistance of the matrix. At the same time, the hydroxymethyl groups at both ends inhibit the reaction of the carboxyl groups at the chain ends with isocyanate, thereby improving the hydrophilicity. Triethylamine is a neutralizing agent that can convert the carboxyl groups in the system into carboxyl groups to form anions. N-(β-aminoethyl)-γ-aminopropyltrimethyl(ethyl)oxysilane can add siloxane to the cement system. At the same time, it has hydroxyl and amino groups, and can form intramolecular hydrogen bonds with organic matter to increase adhesion.
[0035] Preferably, the mass ratio of isophorone diisocyanate, polyethylene glycol, dimethylol propionic acid, triethylamine, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and distilled water is 80-85:95-105:8-12:3-5:2-3:40-50, preferably 84:100:10:4:2.5:45.
[0036] Preferably, the N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane includes N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and N-(β-aminoethyl)-γ-aminopropyltriethoxysilane.
[0037] Preferably, the temperature of the first heating and stirring reaction in step (1) is 55-65° C., preferably 60° C.; and the reaction time is 2-4 h, preferably 3 h.
[0038] Preferably, the temperature of the first heating and stirring reaction in step (2) is 65-75° C., preferably 70° C.; and the reaction time is 3-5 h, preferably 4 h.
[0039] Preferably, in step (3), the temperature of the reaction system is first lowered to 40-50°C, preferably 45°C, and then triethylamine is added. The reaction time is 0.5-1h, preferably 0.8h.
[0040] Preferably, the temperature of the fourth stirring reaction in step (4) is the same as that in step (3), which is 40 to 50° C., preferably 45° C., and the reaction time is 2 to 4 hours, preferably 3 hours.
[0041] Preferably, the temperature of the fifth stirring reaction in step (5) is 30-40° C., preferably 35° C.; the reaction time is 0.5-1.5 h, preferably 1 h.
[0042] In one or more embodiments, the rapid hardening and early strength cement is one or more of aluminate cement, sulphoaluminate cement and magnesium phosphate cement, preferably sulphoaluminate cement. The grade of the rapid hardening and early strength cement is ≥52.5, and the specific surface area is ≤400m 2 / kg, initial setting time ≥45min, final setting time ≤390min, MgO content ≤5%, C3A content ≤8%, chloride ion content ≤0.06%, loss on ignition ≤3%.
[0043] In one or more embodiments, the defoamer is an organosilicon defoamer and / or a polyether defoamer, preferably a polyether defoamer. The defoamer can effectively eliminate bubbles generated during the stirring process of the coating, reduce porosity, improve coating density, and reduce cracking.
[0044] In one or more embodiments, the water reducer is one or more of a polycarboxylate water reducer, a naphthalene water reducer, a melamine water reducer and a melamine water reducer, preferably a naphthalene water reducer. The water reducer can improve the workability of the coating, regulate the fluidity of the coating, and ensure that the coating can complete self-leveling on the plane and ensure that there is no hanging on the vertical surface.
[0045] In one or more embodiments, the early strength agent is one or more of calcium formate, calcium silicate, lithium carbonate, lithium sulfate and lithium chloride, preferably lithium sulfate. The early strength agent can further promote the rapid hardening and early strength of the coating and reduce the sagging and drying shrinkage of the coating.
[0046] A second typical embodiment of the present invention provides a method for preparing the above-mentioned high-toughness and high-durability marine concrete protective coating, comprising:
[0047] Mix the anionic water-based polyurethane and mixing water evenly according to the ratio, then add the fast-hardening and early-strength cement, mix evenly, and add the defoamer, water-reducing agent and early-strength agent during the stirring process.
[0048] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0049] Example 1
[0050] A high-toughness and high-durability marine engineering concrete protective coating, the raw materials of which include: 100 parts of fast-hardening and early-strength cement (sulfoaluminate cement), 16.67 parts of anionic water-based polyurethane, 0.3 parts of defoamer (polyether defoamer), 0.8 parts of water reducer (naphthalene-based water reducer), 0.3 parts of early-strength agent (lithium sulfate), and 28.34 parts of mixing water.
[0051] Wherein, the preparation method of anionic waterborne polyurethane comprises:
[0052] (1) 84 g of isophorone diisocyanate and 100 g of polyethylene glycol were added to an overhead stirrer and heated and stirred at 60° C. for 3 h at a stirring rate of 500 r / min;
[0053] (2) Add 10 g of dihydroxymethylpropionic acid to the reaction system of step (1), heat and stir, the heating temperature is 70° C., the reaction time is 4 h, and the stirring rate is 200 r / min.
[0054] (3) The temperature of the reaction system in step (2) was lowered to 45°C, 4 g of triethylamine was added, and the reaction was stirred for 0.8 h.
[0055] (4) Then, 2.5 g of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane was added to the reaction system of step (3) and the reaction time was 3 h.
[0056] (5) Add 45 g of distilled water to the reaction system of step (4), the reaction temperature is 35° C., the reaction time is 1 h, and the reaction rate is 2000 r / min. Finally, an anionic water-based polyurethane emulsion is obtained, which is sealed in a glass bottle and used as needed.
[0057] The preparation method of the above-mentioned high-toughness and high-durability marine engineering concrete protective coating is:
[0058] Mix the anionic water-based polyurethane and mixing water evenly according to the ratio, stir for 3 minutes to obtain a mixed liquid, then add the fast-hardening and early-strength cement, mix evenly, stir for 3 minutes, and add the defoamer, water reducer and early-strength agent during the stirring process to finally form a uniform slurry.
[0059] Example 2
[0060] A high-toughness and high-durability marine engineering concrete protective coating, the raw materials of which include: 100 parts of fast-hardening and early-strength cement (sulfoaluminate cement), 33.33 parts of anionic water-based polyurethane, 0.6 parts of defoamer (polyether defoamer), 0.6 parts of water reducer (naphthalene-based water reducer), 0.6 parts of early-strength agent (lithium sulfate), and 16.67 parts of mixing water.
[0061] The preparation method of the anionic waterborne polyurethane and the preparation method of the high-toughness and high-durability marine concrete protective coating are the same as those in Example 1.
[0062] Example 3
[0063] A high-toughness and high-durability marine engineering concrete protective coating, the raw materials of which include: 100 parts of fast-hardening and early-strength cement (sulfoaluminate cement), 50 parts of anionic water-based polyurethane, 1 part of defoamer (polyether defoamer), 0.2 parts of water reducer (naphthalene-based water reducer), 1 part of early-strength agent (lithium sulfate), and 5 parts of mixing water.
[0064] The preparation method of the anionic waterborne polyurethane and the preparation method of the high-toughness and high-durability marine concrete protective coating are the same as those in Example 1.
[0065] Comparative Example 1
[0066] A marine engineering concrete protective coating, the raw materials of which include: 100 parts of fast-hardening and early-strength cement (sulfoaluminate cement), 0 parts of defoaming agent (polyether defoaming agent), 1 part of water reducing agent (naphthalene series water reducing agent), 0.2 parts of early-strength agent (lithium sulfate), and 40 parts of mixing water.
[0067] The preparation method of the protective coating is the same as that of Example 1.
[0068] Comparative Example 2
[0069] A marine engineering concrete protective coating, the raw materials of which include: 100 parts of fast-hardening and early-strength cement (sulfoaluminate cement), 50 parts of anionic water-based polyurethane, 1 part of defoamer (polyether defoamer), 0.2 parts of water reducer (naphthalene-based water reducer), 1 part of early-strength agent (lithium sulfate), and 5 parts of mixing water.
[0070] The preparation method of the anionic waterborne polyurethane is different from that of the anionic waterborne polyurethane in Example 1, and step (4) is not added.
[0071] The preparation method of anionic waterborne polyurethane comprises:
[0072] (1) 84 g of isophorone diisocyanate and 100 g of polyethylene glycol were added to an overhead stirrer and heated and stirred at 60° C. for 3 h at a stirring rate of 500 r / min;
[0073] (2) Add 10 g of dihydroxymethylpropionic acid to the reaction system of step (1), heat and stir, the heating temperature is 70° C., the reaction time is 4 h, and the stirring rate is 200 r / min.
[0074] (3) The temperature of the reaction system in step (2) was lowered to 45°C, 4 g of triethylamine was added, and the reaction was stirred for 0.8 h.
[0075] (4) Add 45 g of distilled water to the reaction system of step (3), the reaction temperature is 35° C., the reaction time is 1 h, and the reaction rate is 2000 r / min. Finally, an anionic water-based polyurethane emulsion is obtained, which is sealed in a glass bottle and used as needed.
[0076] The preparation method of the protective coating is the same as that of Example 1.
[0077] Comparative Example 3
[0078] A marine engineering concrete protective coating, the raw materials of which include: 100 parts of ordinary Portland cement, 50 parts of anionic water-based polyurethane, 1 part of defoamer (polyether defoamer), 0 parts of water reducer (naphthalene series water reducer), 1 part of early strength agent (lithium sulfate), and 5 parts of mixing water.
[0079] The preparation method of the anionic waterborne polyurethane and the preparation method of the marine engineering concrete protective coating are the same as those in Example 1.
[0080] Comparative Example 4
[0081] A marine engineering concrete protective coating, the raw materials of which include: 100 parts of fast-hardening and early-strengthening cement (sulfoaluminate cement), 50 parts of commercially available anionic water-based polyurethane, 1 part of defoamer (polyether defoamer), 0.2 parts of water reducer (naphthalene-based water reducer), 1 part of early-strengthening agent (lithium sulfate), and 5 parts of mixing water.
[0082] Experimental Example 1
[0083] According to the national standards GB / T 16777-2008 "Test methods for building waterproof coatings", GB / T 23445-2009 "Polymer cement waterproof coatings", GB / T 528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber" and GB / T 50082-2009 "Test methods for long-term and durability of ordinary concrete", the tensile strength, bonding strength, carbonization resistance, chloride ion corrosion resistance and water pressure resistance of Examples 1 to 3 and Comparative Examples 1 to 4 were tested. The results of the tensile strength of the marine concrete protective coating after 7 days are as follows: Figure 1 The results of the 7-day bond strength of the marine concrete protective coating are shown in Figure 2 As shown in the figure, the carbonization depth of the concrete substrate after coating the marine concrete protective coating is 28 Figure 3 As shown in Figure 2, the results of the anti-permeability of the mortar matrix after coating the marine concrete protective coating are as follows: Figure 4 As shown in Figure 2, the results of the sulfuric acid corrosion resistance of the mortar matrix after coating the marine concrete protective coating are as follows: Figure 5 shown.
[0084] In Examples 1 to 3 and Comparative Examples 1 to 4, the prepared marine concrete protective coatings are used to test the tensile properties of the specimens, which are stored in a curing room (T = 20 ± 5 ° C, RH = 60%) after molding and cured to the corresponding age; and the specimens used to test the bonding and durability properties need to be coated on the concrete surface according to the standard, placed in a curing room (T = 20 ± 5 ° C, RH = 60%) and cured to the corresponding age before conducting relevant tests.
[0085] Depend on Figure 1 and Figure 2It can be seen that with the increase of the amount of anionic waterborne polyurethane, the tensile strength and bonding strength of the coating continue to increase, reaching up to 6.81MPa and 2.9MPa respectively. However, the tensile strength and bonding strength of the coating without anionic waterborne polyurethane do not meet the standard requirements. Compared with the coating with commercial anionic waterborne polyurethane, the tensile strength and tensile strength are increased by 45% and 190% respectively. Compared with the coating with ordinary Portland cement, the tensile strength and tensile strength are increased by 84% and 163% respectively. In addition, the anionic waterborne polyurethane prepared in Comparative Example 2 is not mixed with N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, resulting in reduced mechanical properties, especially a 60% reduction in bonding performance. This fully illustrates that the coating of the present invention has excellent toughness and good compatibility with the concrete matrix.
[0086] Depend on Figures 3 to 5 It can be seen that, compared with Examples 1 to 3 and Comparative Example 1, due to the formation of a dense and uniform three-dimensional interpenetrating polymer network structure between the anionic waterborne polyurethane prepared by the present invention and the sulphoaluminate cement, the coating's resistance to chloride ion erosion, water penetration, carbonization and sulfuric acid erosion is improved with the increase of the anionic waterborne polyurethane dosage. Comparative Example 3 and Comparative Example 2 show that due to the introduction of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane in the preparation process of the anionic waterborne polyurethane, the adhesion between the coating and the substrate is enhanced, thereby enhancing the coating's resistance to chloride ion erosion, water penetration, carbonization and sulfuric acid erosion. Comparative Example 3 and Comparative Example 3 show that due to the slow hydration of ordinary silicate cement, it does not have a synergistic effect with the anionic waterborne polyurethane film, resulting in the failure to form a mutually penetrating three-dimensional network interpenetrating structure, thereby reducing the coating's resistance to chloride ion erosion, water penetration, carbonization and sulfuric acid erosion. By comparing Example 3 with Comparative Example 4, it can be seen that since the commercially available anionic waterborne polyurethane has a single functional group, few reaction sites, and weak cross-linking ability, the coating's resistance to chloride ion corrosion, water penetration, carbonization, and sulfuric acid corrosion is reduced.
[0087] In summary, the protective coating of the present invention can give full play to the respective advantages of polymers and cement, firmly adhere to the concrete matrix, and form a continuous and mutually penetrating polymer network structure inside the system, so as to achieve the requirements of no sag, high toughness, high durability and low shrinkage of the coating, and is suitable for the repair and protection projects of marine concrete structures such as bridges, wind power towers, public buildings, etc. in coastal environments.
[0088] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high-toughness, high-durability marine engineering concrete protective coating, characterized in that: The raw materials include, by weight: 95-105 parts of fast-hardening and early-strengthening cement, 1-50 parts of anionic water-based polyurethane, 0-1 parts of defoaming agent, 0.2-1 parts of water reducing agent, 0.1-1 parts of early-strengthening agent, and 5-40 parts of mixing water; The preparation method of the anionic waterborne polyurethane comprises: (1) isophorone diisocyanate and polyethylene glycol are uniformly mixed and subjected to a first heating and stirring reaction; (2) adding dimethylolpropionic acid to the reaction system of step (1) and performing a second heating and stirring reaction; (3) adding triethylamine to the reaction system of step (2) and performing a third stirring reaction; (4) adding N-(β-aminoethyl)-γ-aminopropyltrimethyl(ethyl)oxysilane to the reaction system of step (3) and performing a fourth stirring reaction; (5) Finally, distilled water is added to the reaction system of step (4) and the reaction is stirred for the fifth time to finally obtain anionic waterborne polyurethane; The rapid hardening and early strength cement is one or more of aluminate cement, sulphoaluminate cement and magnesium phosphate cement; The mass ratio of isophorone diisocyanate, polyethylene glycol, dimethylol propionic acid, triethylamine, N-(β-aminoethyl)-γ-aminopropyltrimethyl(ethyl)oxysilane and distilled water is 80-85:95-105:8-12:3-5:2-3:40-50; The temperature of the first heating and stirring reaction in step (1) is 55-65°C; the reaction time is 2-4 h; The temperature of the second heating and stirring reaction in step (2) is 65-75°C; the reaction time is 3-5 h; In step (3), the temperature of the reaction system is first lowered to 40-50°C, and then triethylamine is added. The reaction time is 0.5-1 h. The temperature of the fourth stirring reaction in step (4) is the same as that in step (3), that is, 40-50° C., and the reaction time is 2-4 h; The temperature of the fifth stirring reaction in step (5) is 30-40°C; the reaction time is 0.5-1.5 h; A dense and uniform three-dimensional interpenetrating polymer network structure is formed between anionic waterborne polyurethane and rapid-hardening and early-strength cement.
2. The high-toughness, high-durability marine concrete protective coating according to claim 1, characterized in that: The mass ratio of isophorone diisocyanate, polyethylene glycol, dimethylol propionic acid, triethylamine, N-(β-aminoethyl)-γ-aminopropyltrimethyl(ethyl)oxysilane and distilled water is 84:100:10:4:2.5:
45.
3. The high-toughness, high-durability marine concrete protective coating according to claim 1, characterized in that: The temperature of the first heating and stirring reaction in step (1) is 60°C; the reaction time is 3 h; Alternatively, the temperature of the second heating and stirring reaction in step (2) is 70° C. and the reaction time is 4 h.
4. The high-toughness, high-durability marine concrete protective coating according to claim 1, characterized in that: In step (3), the temperature of the reaction system is first lowered to 45°C, and then triethylamine is added. The reaction time is 0.8 h. Alternatively, the temperature of the fourth stirring reaction in step (4) is the same as that in step (3), that is, 45° C., and the reaction time is 3 h; Alternatively, the temperature of the fifth stirring reaction in step (5) is 35° C. and the reaction time is 1 h.
5. The high-toughness, high-durability marine concrete protective coating according to claim 1, characterized in that: The rapid hardening and early strength cement is sulphoaluminate cement.
6. The high-toughness, high-durability marine concrete protective coating according to claim 1, characterized in that: The defoamer is an organosilicon defoamer and / or a polyether defoamer.
7. The high-toughness, high-durability marine concrete protective coating according to claim 6, characterized in that: The defoamer is a polyether defoamer.
8. The high-toughness, high-durability marine concrete protective coating according to claim 1, characterized in that: The water reducer is one or more of a polycarboxylic acid water reducer, a naphthalene water reducer, a melamine water reducer and a melamine water reducer.
9. The high-toughness, high-durability marine concrete protective coating according to claim 8, characterized in that: The water reducer is a naphthalene-based water reducer.
10. The high-toughness, high-durability marine concrete protective coating according to claim 1, characterized in that: The early strength agent is one or more of calcium formate, calcium silicate, lithium carbonate, lithium sulfate and lithium chloride.
11. The high-toughness, high-durability marine concrete protective coating according to claim 10, characterized in that: The early strength agent is lithium sulfate.
12. A method for preparing a high-toughness and high-durability marine concrete protective coating according to any one of claims 1 to 11, characterized in that: include: Mix the anionic water-based polyurethane and mixing water evenly according to the ratio, then add the fast-hardening and early-strength cement, mix evenly, and add the defoamer, water-reducing agent and early-strength agent during the stirring process.