A plating hole filling agent for LTCC and its preparation method and application
By using the prepared electroplating pore filler in the LTCC filter to fill the pores on the ceramic surface, the plating diffusion problem caused by the spiral corner process is solved, and the insulation resistance and stability of the product are significantly improved, and electrode conduction and ceramic damage are avoided.
Patent Information
- Application Number
- CN202410378945.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-03-29
AI Technical Summary
During the preparation of 5G LTCC filters, the pore problems caused by the spiral corner process affect the subsequent electroplating process, resulting in electroplating diffusion and affecting product quality.
Using an electroplating pore filler for LTCC, including toluene, anhydrous ethanol, isopropanol, butanol, dispersant, binder, film forming additive and silicone oil, the pore filler is prepared by stirring and the The ceramics treated with piping corners are immersed in the pore filler for surface filling to form a protective layer to prevent the electroplating solution from penetrateing into the pores.
The occurrence of electroplating diffusion is completely avoided, the electrode conductivity and ceramic breakage rate are reduced, the insulation resistance is significantly improved, and the product quality is ensured.
Smart Images

Figure CN118271914B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hole filling slurry, and in particular to an electroplating hole filling agent for LTCC and a preparation method and application thereof. Background Art
[0002] Low Temperature Co-fired Ceramic (LTCC) technology is a process that uses silver as a conductor to fill and print on the green embryo thin strip after the powder end is made into a green embryo through slurry casting, and then the internal circuit layers are interconnected through lamination. Through three-dimensional circuit design, passive electronic devices with harmony, suppression and anti-interference are realized in high-frequency applications. Passive devices must be soldered on PCB boards for end customers to combine with other devices and function. Therefore, the last two processes of passive devices must include trimming the edge corners and electroplating nickel tin processes to help the filter devices be soldered on the circuit board.
[0003] The rolling process is a process of grinding the four corners of the product into an arc shape with an R angle by friction between the products, and then grinding and polishing with alumina powder and water to make the appearance refined. Electroplating is a process of placing the sintered finished products, steel balls and zirconium balls in a drum and immersing them in the electroplating solution for the rolling process, and using the rolling collision mechanism to plate the outer electrodes with nickel and tin. The two process steps use the collision principle between products or between products and hard objects to achieve the purpose of the process. After the rolling process has knocked out pores on the surface of the product, when it comes to the electroplating process, the electroplating solution is rich in conductive liquid that is easily adsorbed and locked in the surface pores, and the current induces the phenomenon of electroplating diffusion during electroplating.
[0004] In order to solve the problem of pores in LTCC materials caused by rolling corners, which affects subsequent electroplating, the commonly used technology is to reduce the rotation speed of the drum and reduce the number of balls put into the drum, or put in soft plastic balls for buffering during electroplating. However, these methods can only reduce the probability of the occurrence of holes, and cannot completely avoid the occurrence of electroplating diffusion, which will still affect the quality after electroplating. How to solve the problem of pores in LTCC materials caused by rolling corners, which affects subsequent electroplating, is one of the key issues that need to be solved in the field of 5G LTCC filter preparation. Summary of the invention
[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a plating hole filling agent for LTCC and a preparation method and application thereof, so as to solve the problem that during the preparation of the existing 5G LTCC filter, due to the appearance of pores in the LTCC material during the rolling corner process, electroplating diffusion occurs in the subsequent electroplating, affecting the quality of the obtained LTCC filter.
[0006] The technical solution of the present invention to solve the above technical problems is as follows:
[0007] An electroplating hole filling agent for LTCC, comprising the following raw materials in parts by weight:
[0008] 40-70 parts of toluene, 20-40 parts of anhydrous ethanol, 6-14 parts of isopropanol, 3-7 parts of butanol, 0.5-2 parts of dispersant, 5-15 parts of binder, 3-8 parts of film-forming aid and 0.01-0.08 parts of silicone oil.
[0009] The beneficial effects of the present invention are as follows: the present invention provides an electroplating hole-filling agent for LTCC, by immersing the low-temperature co-fired ceramic in the hole-filling agent for surface filling after the rolling corner process, and then performing the electroplating process, the hole-filling agent can protect the electroplating solution from not easily penetrating into the pores, and the probability of electroplating diffusion caused by residual electroplating solution can be completely avoided. At the same time, a protective layer can be formed between the product and the zirconium ball, avoiding the possibility of ceramic damage during the electroplating process.
[0010] Further, the following raw materials are included in parts by weight:
[0011] 50-60 parts of toluene, 25-35 parts of anhydrous ethanol, 8-12 parts of isopropanol, 4-6 parts of butanol, 0.8-1.5 parts of dispersant, 8-12 parts of binder, 4-6 parts of film-forming aid and 0.05-0.08 parts of silicone oil.
[0012] The beneficial effect of adopting the above further technical solution is: the present invention can effectively solve the occurrence of electrode conductivity and ceramic breakage rate by further adjusting the content of each component in the raw material composition. The electrode conductivity can be reduced from 60% without the hole filling agent treatment to 0%, and the ceramic breakage rate can also be reduced from 4.5% to 0%, completely avoiding the defects of mutual conduction of electrodes and ceramic breakage. Among them, toluene, anhydrous ethanol, isopropanol and butanol not only effectively improve the dispersion effect of the prepared hole filling agent through their own high solubility, have the function of adjusting the viscosity of the hole filling agent, but also effectively improve the volatilization point of the mixed solvent through mixing, slow down the degree of solvent volatilization, and improve the stability of the prepared hole filling agent at room temperature.
[0013] Further, the following raw materials are included in parts by weight:
[0014] 55 parts of toluene, 30 parts of anhydrous ethanol, 10 parts of isopropanol, 5 parts of butanol, 1 part of dispersant, 10 parts of binder, 5 parts of film-forming aid and 0.08 parts of silicone oil.
[0015] The beneficial effects of adopting the above further technical solution are as follows: the present invention can completely avoid the defects of mutual conduction of electrodes and ceramic damage by further optimizing and adjusting the content of each component in the raw material composition, and effectively improve the insulation resistance of the obtained product, which is 2.3×10 9 Ω·cm significantly increased to 1.3×10 11 Ω·cm.
[0016] Furthermore, the dispersant is prepared by mixing an anionic hydrophilic dispersant with acid radicals and an alkali metal salt dispersant in a volume ratio of 0.5-1.5:0.5-1.5; the anionic hydrophilic dispersant with acid radicals includes any one of sodium polyvinyl sulfonate and sodium polyacrylate; the alkali metal salt dispersant includes any one of sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate.
[0017] The beneficial effect of adopting the above further technical solution is: the present invention adopts the method of preparing the mixed dispersant by using anionic hydrophilic dispersant with acid radical and alkali metal salt dispersant, which not only effectively prevents the sedimentation of the pore filling agent, but also plays a role in increasing the storage stability of the pore filling agent.
[0018] Furthermore, the binder is polyvinyl butyral with a molecular weight of 55,000 to 120,000.
[0019] The beneficial effect of adopting the above further technical scheme is: the present invention adds polyvinyl butyral ester as a binder, which plays a film-forming role in the prepared pore-filling agent. By adjusting its added amount, the use conditions of low-temperature co-fired ceramics with different degrees of damage can be effectively met, avoiding the occurrence of double-bonding material phenomenon.
[0020] Furthermore, the film-forming aid is an organic compound with a diester structure.
[0021] Furthermore, the film-forming aid is an OE300 film-forming aid.
[0022] The beneficial effects of adopting the above-mentioned further technical scheme are as follows: the present invention adds OE300 type film-forming aid, which is combined with a binder to effectively improve the film-forming hardness of the pore filling agent, improve the pore filling effect of low-temperature co-fired ceramics, improve the wear resistance and temperature and humidity resistance of the filling membrane, and effectively inhibit the generation of foam in the pore filling agent.
[0023] Furthermore, the silicone oil is dimethyl silicone oil.
[0024] The beneficial effect of adopting the above-mentioned further technical scheme is as follows: the present invention provides inorganic silicon dioxide by adding dimethyl silicone oil, so that a silicon film of a certain thickness is formed on the ceramic body to fill the tiny holes and cracks on the outside of the ceramic product, and the insulation resistance of the electroplated product is improved through the good insulation, high mechanical strength and corrosion resistance of the silicon film itself.
[0025] The preparation method of the electroplating hole filling agent for LTCC comprises the following steps:
[0026] The toluene, anhydrous ethanol, isopropanol, butanol and dispersant are mixed and stirred for the first time; then a binder and a film-forming aid are added and stirred for the second time; finally silicone oil is added and stirred for the third time to obtain the product.
[0027] The beneficial effects of the present invention are as follows: the present invention effectively improves the uniformity of the pore filling agent by mixing and stirring the raw materials in batches, adopts different temperatures, rotation speeds and stirring times, and effectively controls the viscosity of the prepared pore filling agent to be between 100 and 400 cps.
[0028] Furthermore, the first stirring temperature is 28-32° C., the rotation speed is 40-60 rpm, and the time is 1-3 h.
[0029] Preferably, the first stirring temperature is 30° C., the rotation speed is 50 rpm, and the time is 2 h.
[0030] The beneficial effect of adopting the above further technical solution is that by mixing four different solvents with the dispersant and then stirring, the solvents can be fully dissolved and the dispersibility of the subsequent polymer compound added can be improved.
[0031] Furthermore, the second stirring temperature is 75-85° C., the rotation speed is 200-400 rpm, and the time is 10-15 hours.
[0032] Preferably, the second stirring temperature is 80° C., the rotation speed is 300 rpm, and the time is 12 h.
[0033] The beneficial effects of adopting the above further technical solution are: through stirring at a higher temperature and speed, the added polymer powder binder is completely dissolved in the solvent, and the film-forming aid and the binder are fully blended, thereby improving the subsequent film-forming effect.
[0034] Furthermore, the third stirring is performed at a temperature of 23 to 27° C., a rotation speed of 200 to 400 rpm, and a time of 3 to 5 hours.
[0035] Preferably, the third stirring temperature is 25° C., the rotation speed is 300 rpm, and the time is 4 hours.
[0036] The beneficial effect of adopting the above further technical solution is: finally adding silicone oil, and through long-term mixing and stirring, the silicone oil and the solvent are fully mixed with each other, the viscosity of the pore filling agent is improved, and the insulation, mechanical strength and corrosion resistance of the silicon film produced by subsequent processing are improved.
[0037] The above-mentioned electroplating hole-filling agent for LTCC is used in the preparation of LTCC filter.
[0038] The beneficial effects of the present invention are as follows: the present invention provides a hole-filling agent for the preparation of LTCC filters, thereby effectively solving the phenomenon of electroplating diffusion caused by the rolling angle process during the electroplating process, preventing the occurrence of defects such as mutual conduction between electrodes and ceramic damage, and effectively improving the insulation resistance of the product.
[0039] Furthermore, the application of the above-mentioned electroplating hole filling agent for LTCC in the preparation of LTCC filter includes the following steps: immersing the low-temperature co-fired ceramic body after the rolling corner process in the hole filling agent, taking it out, drying it, sintering it, and finally performing the electroplating process to obtain it.
[0040] The beneficial effect of adopting the above-mentioned further technical scheme is as follows: the present invention adds a hole filling process after the edge rolling process, and solidifies the silicon film by drying, and then fuses the silicon dioxide with the external electrode by sintering, so that the silver metal of the external electrode of the product after sintering can be exposed, thereby avoiding the influence of the original electroplating process conditions during subsequent electroplating, and filling the pores with silicon dioxide on the surface of the ceramic body, thereby avoiding the electroplating diffusion phenomenon caused by the electroplating solution penetrating into the ceramic pores.
[0041] Furthermore, the soaking conditions are: shaking the sintered low-temperature co-fired ceramic body every 20 to 40 seconds, and the soaking time is 10-30 minutes; the drying temperature is 100-200°C, and the time is 30-50 minutes; the sintering temperature is 600-700°C, and the time is 5-15 minutes.
[0042] Preferably, the soaking conditions are: shaking the sintered low-temperature co-fired ceramic body every 30 seconds, and the soaking time is 20 minutes; the drying temperature is 160°C, and the time is 40 minutes; the sintering temperature is 650°C, and the time is 10 minutes.
[0043] The present invention has the following beneficial effects:
[0044] The present invention provides an electroplating hole filling agent for LTCC and a preparation method thereof. The preparation method is simple, the raw material source is wide, and it is easy to be industrially produced on a large scale. The prepared electroplating hole filling agent for LTCC can be added to the hole filling process after the low temperature co-fired ceramic edge rolling, effectively solving the electroplating diffusion phenomenon caused by the edge rolling process in the electroplating process, preventing the occurrence of defects such as mutual conduction of electrodes and ceramic damage, and effectively improving the insulation resistance of the prepared product. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1This is a sample picture of the control group in Experimental Example 1 where the electroplating diffusion phenomenon occurs;
[0046] Figure 2 It is a schematic diagram of the principle of electroplating diffusion phenomenon in the control group of Experimental Example 1;
[0047] Figure 3 This is a sample without electroplating diffusion phenomenon obtained by using the hole filling agent obtained in Example 8 in Experimental Example 1;
[0048] Figure 4 This is a schematic diagram of the principle of using the hole filling agent obtained in Example 8 in Experimental Example 1 to prepare a sample without electroplating diffusion phenomenon;
[0049] Figure 5 This is a sample picture of white spot damage after electroplating in the control group of Experimental Example 1;
[0050] Figure 6 This is a sample without white spot damage obtained by using the pore filling agent obtained in Example 8 in Test Example 1. DETAILED DESCRIPTION
[0051] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0052] Embodiment 1:
[0053] An electroplating hole filling agent for LTCC, comprising the following raw materials in parts by weight:
[0054] 55 parts of toluene, 30 parts of anhydrous ethanol, 10 parts of isopropanol, 5 parts of butanol, 1 part of a mixed dispersant prepared by mixing sodium polysulfonate and sodium hexametaphosphate in a volume ratio of 1:1, 10 parts of polypropylene butyral with a molecular weight of 80,000, 5 parts of OE300 type film-forming aid and 0.01 parts of dimethyl silicone oil.
[0055] The preparation method of the electroplating hole filling agent for LTCC comprises the following steps:
[0056] (1) Pour toluene, anhydrous ethanol, isopropanol, butanol and mixed dispersant into a stainless steel stirring barrel and stir at 30°C and 50 rpm for 2 h;
[0057] (2) Add polypropylene butyral and OE300 film-forming aid into a stirring barrel and stir at 80°C and 300 rpm for 12 h;
[0058] (3) Add dimethyl silicone oil into a stirring barrel, stir at 25° C. and 300 rpm for 4 h to obtain the product.
[0059] Embodiment 2:
[0060] An electroplating hole filling agent for LTCC, comprising the following raw materials in parts by weight:
[0061] 55 parts of toluene, 30 parts of anhydrous ethanol, 10 parts of isopropanol, 5 parts of butanol, 1 part of a mixed dispersant prepared by mixing sodium polysulfonate and sodium hexametaphosphate in a volume ratio of 1:1, 10 parts of polypropylene butyral with a molecular weight of 80,000, 5 parts of OE300 type film-forming aid and 0.02 parts of dimethyl silicone oil.
[0062] The preparation method of the electroplating hole filling agent for LTCC comprises the following steps:
[0063] (1) Pour toluene, anhydrous ethanol, isopropanol, butanol and mixed dispersant into a stainless steel stirring barrel and stir at 30°C and 50 rpm for 2 h;
[0064] (2) Add polypropylene butyral and OE300 film-forming aid into a stirring barrel and stir at 80°C and 300 rpm for 12 h;
[0065] (3) Add dimethyl silicone oil into a stirring barrel, stir at 25° C. and 300 rpm for 4 h to obtain the product.
[0066] Embodiment 3:
[0067] An electroplating hole filling agent for LTCC, comprising the following raw materials in parts by weight:
[0068] 55 parts of toluene, 30 parts of anhydrous ethanol, 10 parts of isopropanol, 5 parts of butanol, 1 part of a mixed dispersant prepared by mixing sodium polyvinyl sulfonate and sodium hexametaphosphate in a volume ratio of 1:1, 10 parts of polypropylene butyral with a molecular weight of 80,000, 5 parts of OE300 type film-forming aid and 0.03 parts of dimethyl silicone oil.
[0069] The preparation method of the electroplating hole filling agent for LTCC comprises the following steps:
[0070] (1) Pour toluene, anhydrous ethanol, isopropanol, butanol and mixed dispersant into a stainless steel stirring barrel and stir at 30°C and 50 rpm for 2 h;
[0071] (2) Add polypropylene butyral and OE300 film-forming aid into a stirring barrel and stir at 80°C and 300 rpm for 12 h;
[0072] (3) Add dimethyl silicone oil into a stirring barrel, stir at 25° C. and 300 rpm for 4 h to obtain the product.
[0073] Embodiment 4:
[0074] An electroplating hole filling agent for LTCC, comprising the following raw materials in parts by weight:
[0075] 55 parts of toluene, 30 parts of anhydrous ethanol, 10 parts of isopropanol, 5 parts of butanol, 1 part of a mixed dispersant prepared by mixing sodium polysulfonate and sodium hexametaphosphate in a volume ratio of 1:1, 10 parts of polypropylene butyral with a molecular weight of 80,000, 5 parts of OE300 type film-forming aid and 0.04 parts of dimethyl silicone oil.
[0076] The preparation method of the electroplating hole filling agent for LTCC comprises the following steps:
[0077] (1) Pour toluene, anhydrous ethanol, isopropanol, butanol and mixed dispersant into a stainless steel stirring barrel and stir at 30°C and 50 rpm for 2 h;
[0078] (2) Add polypropylene butyral and OE300 film-forming aid into a stirring barrel and stir at 80°C and 300 rpm for 12 h;
[0079] (3) Add dimethyl silicone oil into a stirring barrel, stir at 25° C. and 300 rpm for 4 h to obtain the product.
[0080] Embodiment 5:
[0081] An electroplating hole filling agent for LTCC, comprising the following raw materials in parts by weight:
[0082] 55 parts of toluene, 30 parts of anhydrous ethanol, 10 parts of isopropanol, 5 parts of butanol, 1 part of a mixed dispersant prepared by mixing sodium polyvinyl sulfonate and sodium hexametaphosphate in a volume ratio of 1:1, 10 parts of polypropylene butyral with a molecular weight of 80,000, 5 parts of OE300 type film-forming aid and 0.05 parts of dimethyl silicone oil.
[0083] The preparation method of the electroplating hole filling agent for LTCC comprises the following steps:
[0084] (1) Pour toluene, anhydrous ethanol, isopropanol, butanol and mixed dispersant into a stainless steel stirring barrel and stir at 30°C and 50 rpm for 2 h;
[0085] (2) Add polypropylene butyral and OE300 film-forming aid into a stirring barrel and stir at 80°C and 300 rpm for 12 h;
[0086] (3) Add dimethyl silicone oil into a stirring barrel, stir at 25° C. and 300 rpm for 4 h to obtain the product.
[0087] Embodiment 6:
[0088] An electroplating hole filling agent for LTCC, comprising the following raw materials in parts by weight:
[0089] 55 parts of toluene, 30 parts of anhydrous ethanol, 10 parts of isopropanol, 5 parts of butanol, 1 part of a mixed dispersant prepared by mixing sodium polyvinyl sulfonate and sodium hexametaphosphate in a volume ratio of 1:1, 10 parts of polypropylene butyral with a molecular weight of 80,000, 5 parts of OE300 type film-forming aid and 0.06 parts of dimethyl silicone oil.
[0090] The preparation method of the electroplating hole filling agent for LTCC comprises the following steps:
[0091] (1) Pour toluene, anhydrous ethanol, isopropanol, butanol and mixed dispersant into a stainless steel stirring barrel and stir at 30°C and 50 rpm for 2 h;
[0092] (2) Add polypropylene butyral and OE300 film-forming aid into a stirring barrel and stir at 80°C and 300 rpm for 12 h;
[0093] (3) Add dimethyl silicone oil into a stirring barrel, stir at 25° C. and 300 rpm for 4 h to obtain the product.
[0094] Embodiment 7:
[0095] An electroplating hole filling agent for LTCC, comprising the following raw materials in parts by weight:
[0096] 55 parts of toluene, 30 parts of anhydrous ethanol, 10 parts of isopropanol, 5 parts of butanol, 1 part of a mixed dispersant prepared by mixing sodium polyvinyl sulfonate and sodium hexametaphosphate in a volume ratio of 1:1, 10 parts of polypropylene butyral with a molecular weight of 80,000, 5 parts of OE300 type film-forming aid and 0.07 parts of dimethyl silicone oil.
[0097] The preparation method of the electroplating hole filling agent for LTCC comprises the following steps:
[0098] (1) Pour toluene, anhydrous ethanol, isopropanol, butanol and mixed dispersant into a stainless steel stirring barrel and stir at 30°C and 50 rpm for 2 h;
[0099] (2) Add polypropylene butyral and OE300 film-forming aid into a stirring barrel and stir at 80°C and 300 rpm for 12 h;
[0100] (3) Add dimethyl silicone oil into a stirring barrel, stir at 25° C. and 300 rpm for 4 h to obtain the product.
[0101] Embodiment 8:
[0102] An electroplating hole filling agent for LTCC, comprising the following raw materials in parts by weight:
[0103] 55 parts of toluene, 30 parts of anhydrous ethanol, 10 parts of isopropanol, 5 parts of butanol, 10 parts of a mixed dispersant prepared by mixing sodium polysulfonate and sodium hexametaphosphate in a volume ratio of 1:1, 5 parts of an OE300 film-forming aid and 0.08 parts of dimethyl silicone oil.
[0104] The preparation method of the electroplating hole filling agent for LTCC comprises the following steps:
[0105] (1) Pour toluene, anhydrous ethanol, isopropanol, butanol and mixed dispersant into a stainless steel stirring barrel and stir at 30°C and 50 rpm for 2 h;
[0106] (2) Add polypropylene butyral and OE300 film-forming aid into a stirring barrel and stir at 80°C and 300 rpm for 12 h;
[0107] (3) Add dimethyl silicone oil into a stirring barrel, stir at 25° C. and 300 rpm for 4 h to obtain the product.
[0108] Comparative Example 1:
[0109] An electroplating hole filling agent for LTCC, comprising the following raw materials in parts by weight:
[0110] 55 parts of toluene, 30 parts of anhydrous ethanol, 10 parts of isopropanol, 5 parts of butanol, 1 part of a mixed dispersant prepared by mixing sodium polyvinyl sulfonate and sodium hexametaphosphate in a volume ratio of 1:1, 10 parts of polypropylene butyral with a molecular weight of 80,000, and 5 parts of an OE300 film-forming aid.
[0111] The preparation method of the electroplating hole filling agent for LTCC comprises the following steps:
[0112] (1) Pour toluene, anhydrous ethanol, isopropanol, butanol and mixed dispersant into a stainless steel stirring barrel and stir at 30°C and 50 rpm for 2 h;
[0113] (2) Add polypropylene butyral and OE300 film-forming aid into a stirring barrel, stir at 80° C. and 300 rpm for 12 h to obtain a film-forming agent.
[0114] Comparative Example 2:
[0115] An electroplating hole filling agent for LTCC, comprising the following raw materials in parts by weight:
[0116] 55 parts of toluene, 30 parts of anhydrous ethanol, 10 parts of isopropanol, 5 parts of butanol, 1 part of a mixed dispersant prepared by mixing sodium polyvinyl sulfonate and sodium hexametaphosphate in a volume ratio of 1:1, 10 parts of polypropylene butyral with a molecular weight of 80,000, 5 parts of OE300 type film-forming aid and 0.09 parts of dimethyl silicone oil.
[0117] The preparation method of the electroplating hole filling agent for LTCC comprises the following steps:
[0118] (1) Pour toluene, anhydrous ethanol, isopropanol, butanol and mixed dispersant into a stainless steel stirring barrel and stir at 30°C and 50 rpm for 2 h;
[0119] (2) Add polypropylene butyral and OE300 film-forming aid into a stirring barrel and stir at 80°C and 300 rpm for 12 h;
[0120] (3) Add dimethyl silicone oil into a stirring barrel, stir at 25° C. and 300 rpm for 4 h to obtain the product.
[0121] Comparative Example 3:
[0122] An electroplating hole filling agent for LTCC, comprising the following raw materials in parts by weight:
[0123] 55 parts of toluene, 30 parts of anhydrous ethanol, 10 parts of isopropanol, 5 parts of butanol, 1 part of a mixed dispersant prepared by mixing sodium polysulfonate and sodium hexametaphosphate in a volume ratio of 1:1, 10 parts of polypropylene butyral with a molecular weight of 80,000, 5 parts of OE300 type film-forming aid and 0.10 parts of dimethyl silicone oil.
[0124] The preparation method of the electroplating hole filling agent for LTCC comprises the following steps:
[0125] (1) Pour toluene, anhydrous ethanol, isopropanol, butanol and mixed dispersant into a stainless steel stirring barrel and stir at 30°C and 50 rpm for 2 h;
[0126] (2) Add polypropylene butyral and OE300 film-forming aid into a stirring barrel and stir at 80°C and 300 rpm for 12 h;
[0127] (3) Add dimethyl silicone oil into a stirring barrel, stir at 25° C. and 300 rpm for 4 h to obtain the product.
[0128] Test Example 1: Electroplating experiment and external electrode performance test
[0129] The electroplating hole filling agent for LTCC prepared by the present invention was used for electroplating experiments. The experimental group immersed the low-temperature co-fired ceramic body after the rolling corner process in the hole filling agent, and shook the sintered low-temperature co-fired ceramic body every 30 seconds for immersion, and the immersion time was 20 minutes; after taking out, it was dried at 160°C for 40 minutes, and then sintered at 650°C for 10 minutes, and finally immersed in the electroplating solution to plate nickel and tin metals on the external electrodes to prepare 5G LTCC filters. The control group was used without adding the hole filling agent.
[0130] (1) The experimental results and principle diagram of the sample surface morphology obtained in Example 8 are as follows: Figure 1-Figure 6 shown.
[0131] according to Figure 1-Figure 2 It can be seen that the control group without adding the pore filling agent showed the phenomenon of electroplating diffusion. The electroplating diffusion is caused by the penetration of the electroplating solution into the ceramic pores. The electroplating solution is a solution with extremely low conductivity. If the electroplating solution penetrates into the pores during electroplating, it is easy to cause the electroplated nickel-tin to spread toward the ceramic.
[0132] according to Figure 3-Figure 4 It can be seen that the present invention uses the hole filling process to first perform the hole filling process after the rolling corners, fill the ceramic pores, and then perform the electroplating process, which effectively avoids the occurrence of diffusion reaction. The principle of the process is to first soak the product with the hole filling agent prepared by the present invention, and after completion, the LTCC filter product is protected by the hole filling agent, which can completely solve the probability of electroplating diffusion.
[0133] In the final test packaging process of the LTCC filter manufacturing process, the product is transferred by adjusting the vibration intensity of the track. In this process, the product will collide with the stainless steel or iron track back and forth at a high frequency. The product enters the straight track from the circular turntable, and then the suction nozzle sucks the product and applies downward pressure to complete the overall operation of the test packaging machine. The purpose is to pass the electroplated product through the packaging machine and wrap the electrical good products in the reel paper tape. The overall operation process of this test packaging machine is very likely to cause the product to collide with the hard ground material track at a high degree, resulting in large areas of white spots on the product. Figure 5 The experimental results show that the control group without the pore-filling agent has large areas of white spots and damage. However, the experimental group with the pore-filling agent prepared in Example 8 has a significant protective effect on the appearance of the product, effectively avoiding the occurrence of large-area falling damage on the product.
[0134] (2) Sample performance test
[0135] Test method:
[0136] Electrode diffusion rate: 100 samples were randomly selected for each experimental group, and the number of samples with electrode diffusion was counted to calculate the electrode diffusion rate, which was calculated as follows: electrode diffusion rate = number of electrode diffusion samples / 100 × 100%;
[0137] Maximum diffusion distance: Direct measurement using an optical microscope;
[0138] Damage rate: 100 samples are randomly selected for each experimental group, and the number of samples with appearance damage is counted to calculate the damage rate, which is the number of samples with appearance damage / 100×100%;
[0139] Surface silicon content: X-ray fluorescence spectrometer (XRF) was used to measure the silicon content on the surface of the sample;
[0140] Insulation resistance: Use KEYSIGHT B2985A insulation resistance meter, set 10V, test time 20s, and place the probes at both ends of the end in contact with two different pin electrodes on the outside of the product to measure the insulation resistance.
[0141] The experimental results are shown in Table 1 below.
[0142] Table 1 Sample performance parameters
[0143]
[0144] According to the experimental results in the above table, compared with Comparative Example 1, the electrode diffusion rate, maximum diffusion distance and ceramic breakage rate of the sample treated with the pore filling agent prepared in the embodiment of the present invention are significantly reduced, and the insulation resistance is significantly increased. Among them, the sample treated with the pore filling agent prepared in Example 8 is the best embodiment of the present application, and the electrode diffusion rate, maximum diffusion distance and ceramic breakage rate are all 0, and the insulation resistance reaches 1.3×10 11 When the amount of dimethyl silicone oil added to the pore filling agent reaches 0.09 parts (Comparative Example 2) and 0.10 parts (Comparative Example 3), although the electrode diffusion rate, maximum diffusion distance and ceramic breakage rate of the prepared samples are all 0, the products adhere to each other to form a double adhesive material, which is not suitable for use.
[0145] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An electroplating hole filling agent for LTCC, characterized in that: The invention comprises the following raw materials in parts by weight: 40-70 parts of toluene, 20-40 parts of anhydrous ethanol, 6-14 parts of isopropanol, 3-7 parts of butanol, 0.5-2 parts of dispersant, 5-15 parts of binder, 3-8 parts of film-forming aid and 0.01-0.08 parts of silicone oil; The dispersant is prepared by mixing an anionic hydrophilic dispersant with acid radicals and an alkali metal salt dispersant in a volume ratio of 0.5-1.5:0.5-1.5; the anionic hydrophilic dispersant with acid radicals includes any one of sodium polyvinyl sulfonate and sodium polyacrylate; the alkali metal salt dispersant includes any one of sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate; The binder is polyvinyl butyral with a molecular weight of 55,000 to 120,000; the film-forming aid is an organic compound with a diester structure; and the silicone oil is dimethyl silicone oil.
2. The electroplating hole filling agent for LTCC according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 50-60 parts of toluene, 25-35 parts of anhydrous ethanol, 8-12 parts of isopropanol, 4-6 parts of butanol, 0.8-1.5 parts of dispersant, 8-12 parts of binder, 4-6 parts of film-forming aid and 0.05-0.08 parts of silicone oil.
3. The electroplating hole filling agent for LTCC according to claim 2, characterized in that: The invention comprises the following raw materials in parts by weight: 55 parts of toluene, 30 parts of anhydrous ethanol, 10 parts of isopropanol, 5 parts of butanol, 1 part of dispersant, 10 parts of binder, 5 parts of film-forming aid and 0.08 parts of silicone oil.
4. The method for preparing the electroplating hole filling agent for LTCC according to any one of claims 1 to 3, characterized in that: The following steps are involved: The toluene, anhydrous ethanol, isopropanol, butanol and dispersant are mixed and stirred for the first time; then a binder and a film-forming aid are added and stirred for the second time; finally silicone oil is added and stirred for the third time to obtain the product.
5. The method for preparing the electroplating hole filling agent for LTCC according to claim 4, characterized in that: The temperature of the first stirring is 28-32°C, the rotation speed is 40-60rpm, and the time is 1-3h; the temperature of the second stirring is 75-85°C, the rotation speed is 200-400rpm, and the time is 10-15h; the temperature of the third stirring is 23-27°C, the rotation speed is 200-400rpm, and the time is 3-5h.
6. Use of the electroplating hole-filling agent for LTCC according to any one of claims 1 to 3 in the preparation of LTCC filters.
7. Use of the electroplating hole filling agent for LTCC according to claim 6 in preparing LTCC filters, characterized in that: The method comprises the following steps: soaking the low temperature co-fired ceramic body processed by the rolling corner process in a pore filling agent, taking it out, drying it, sintering it, and finally performing an electroplating process to obtain the product.
8. Use of the electroplating hole filling agent for LTCC according to claim 7 in preparing LTCC filters, characterized in that: The soaking conditions are as follows: shaking the sintered low-temperature co-fired ceramic body every 20 to 40 seconds, and the soaking time is 10-30 minutes; the drying temperature is 100-200°C, and the time is 30-50 minutes; the sintering temperature is 600-700°C, and the time is 5-15 minutes.