Material of sensor wire and integrated multi-point temperature sensor made of the material

By using armored thermocouples and quartz sleeves reinforced with lanthanum, gadolinium, scandium and other components in the temperature sensor, the problems of short service life and poor corrosion resistance of existing temperature sensors in photovoltaic diffusion furnaces are solved, and high accuracy is achieved , Long-life multi-point temperature measurement.

CN118274987BActive Publication Date: 2024-10-22CHONGQING MATERIALS RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410423246.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-09
Publication Date
2024-10-22
Estimated Expiration
2044-04-09

AI Technical Summary

Technical Problem

Existing temperature sensors have short service life and poor corrosion resistance in photovoltaic diffusion furnaces, making it difficult to meet the environmental requirements of high temperature and highly active corrosive media.

Method used

K-type and S-type armored thermocouples reinforced with lanthanum, gadolinium, scandium and other components are used, combined with quartz sleeves and high-temperature resistant inorganic glue to form an integrated multi-point temperature sensor to improve the resistance to high-temperature thermal corrosion and medium corrosion.

Benefits of technology

The stability and service life of the temperature sensor are significantly improved. It can work for a long time in an environment of 1050°C. It has high temperature measurement accuracy and a service life of more than 10 months. It is suitable for the photovoltaic field and other high-temperature industrial fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118274987B_ABST
    Figure CN118274987B_ABST
Patent Text Reader

Abstract

The material of the sensor filament and the integrated multi-point temperature sensor prepared with the material, compared with the prior art, the material has three components of lanthanum, gadolinium and scandium added. The applicant's experiment shows that the integrated multi-point temperature sensor has long-term working stability, and can work for a long time at 1050°C in the complex atmosphere environment of the crystalline silicon growth diffusion furnace in the photovoltaic field, and the service life is more than 10 months, which greatly improves the service life. The sensor is highly integrated, has the advantages of good temperature measurement stability, high measurement accuracy, good corrosion resistance and easy installation, and the maximum operating temperature can reach 1300°C. It can also be promoted and applied to temperature measurement and control in other high-temperature industrial fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sensors, and in particular relates to a material for a sensor filament and an integrated multi-point temperature sensor prepared by using the material. Background Art

[0002] Renewable energy represented by solar photovoltaic power generation technology is one of the technologies with the greatest development potential. Vigorously promoting the photovoltaic industry is of great significance to optimizing the clean energy structure. Photovoltaic equipment is a key development direction in my country's high-end equipment manufacturing field.

[0003] The growth diffusion system in the photovoltaic industry is a key equipment for producing crystalline silicon wafers. The working environment of the photovoltaic diffusion furnace is a long-term temperature of 1050°C, and the instantaneous temperature can be as high as 1200°C. It is also equipped with multiple isothermal zones with a long span and rich in highly active corrosive media. At present, although the existing temperature sensors can measure multi-point temperatures, they have poor corrosion resistance. As the sensor is used for a longer time, its stability decreases, and its service life is low, usually only 4-6 months. Therefore, the development of temperature sensors suitable for photovoltaic diffusion furnaces and meeting the above conditions has become a research focus. Summary of the invention

[0004] The purpose of the present invention is to address the problems existing in the prior art and to propose an integrated multi-point temperature sensor, which enables the temperature sensor to achieve multi-point temperature measurement by inserting multiple armored thermocouples of different lengths into a quartz sleeve; and adding three components of lanthanum, gadolinium and scandium to the positive and negative electrodes of the K-type and S-type armored thermocouples. At the same time, the K-type and S-type thermocouples adopt an armored structure, which improves the high-temperature thermal corrosion resistance and medium corrosion resistance of the integrated multi-point temperature sensor, and improves the working stability and service life of the integrated multi-point temperature sensor.

[0005] To achieve the above object, the present invention provides the following technical solutions.

[0006] Materials for the wire of the integrated multi-point temperature sensor, the wire comprising a wire of a K-type thermocouple or a wire of an S-type thermocouple; the weight proportions of the components in the positive electrode of the wire of the K-type thermocouple are 89.9 to 90.1 parts of nickel, 9.9 to 10.1 parts of chromium, 0.001 to 0.003 parts of lanthanum, 0.001 to 0.003 parts of gadolinium, and 0.001 to 0.003 parts of scandium; the weight proportions of the components in the negative electrode of the wire of the K-type thermocouple are 96.9 to 97.1 parts of nickel, 2.9 to 3.1 parts of silicon, 0.001 to 0.003 parts of lanthanum, 0.001 to 0.003 parts of gadolinium, and 0.001 to 0.003 parts of scandium;

[0007] The weight parts of the components in the positive electrode of the S-type thermocouple are: 89.9-90.1 parts of platinum, 9.9-10.10 parts of rhodium, 0.001-0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.003 parts of scandium. The weight parts of the components in the negative electrode of the S-type thermocouple are: 99.9-100 parts of platinum, 0.001-0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.003 parts of scandium.

[0008] Furthermore, the weight parts of the components in the positive electrode of the K-type thermocouple are 89.950 to 89.971 parts of nickel, 10.020 to 10.040 parts of chromium, 0.003 parts of lanthanum, 0.001 to 0.003 parts of gadolinium, and 0.001 to 0.002 parts of scandium; the weight parts of the components in the negative electrode of the K-type thermocouple are 96.930 to 96.970 parts of nickel, 3.020 to 3.056 parts of silicon, 0.003 parts of lanthanum, 0.001 to 0.003 parts of gadolinium, and 0.001 to 0.002 parts of scandium.

[0009] Furthermore, the weight proportions of the components in the positive electrode of the S-type thermocouple are 89.950 to 89.997 parts of platinum, 9.995 to 10.043 parts of rhodium, 0.003 parts of lanthanum, 0.001 to 0.002 parts of gadolinium, and 0.001 to 0.003 parts of scandium; the weight proportions of the components in the negative electrode of the S-type thermocouple are 99.992 to 99.995 parts of platinum, 0.003 parts of lanthanum, 0.001 to 0.002 parts of gadolinium, and 0.001 to 0.003 parts of scandium.

[0010] The integrated multi-point temperature sensor prepared by using the material comprises a sleeve with one end sealed, and a plurality of armored thermocouples of different lengths, wherein the hot ends of the plurality of armored thermocouples of different lengths are inserted into the sleeve to form a plurality of temperature measurement points, and the armored thermocouples are K-type thermocouples or S-type thermocouples; the pair wires of the S-type thermocouples are inserted into a calcined corundum double-hole ceramic core, and the impurities in the ceramic core are volatilized by calcination, thereby avoiding contamination of the pair wires by impurities at high temperatures, reducing the problems of low temperature measurement accuracy and breakage of the pair wires due to impurity contamination, and improving the service life and temperature measurement accuracy of the integrated multi-point temperature sensor;

[0011] The weight parts of the components in the positive electrode of the K-type thermocouple are: 89.9-90.1 parts of nickel, 9.9-10.1 parts of chromium, 0.001-0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.003 parts of scandium; the weight parts of the components in the negative electrode of the K-type thermocouple are: 96.9-97.1 parts of nickel, 2.9-3.1 parts of silicon, 0.001-0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.003 parts of scandium;

[0012] The weight parts of the components in the positive electrode of the S-type thermocouple are: 89.9-90.1 parts of platinum, 9.9-10.10 parts of rhodium, 0.001-0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.003 parts of scandium. The weight parts of the components in the negative electrode of the S-type thermocouple are: 99.9-100 parts of platinum, 0.001-0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.003 parts of scandium.

[0013] Furthermore, the corundum double-hole ceramic core serves as an insulating carrier of the even wire.

[0014] Furthermore, the cold end of the armored thermocouple extends out of the sleeve mouth, and the wires of the armored thermocouple extend from the cold end and are respectively welded to the compensation wires. Each welding point is wrapped with a heat shrink tube, and the heat shrink tube is used to seal the welding point to ensure the insulation and corrosion resistance of the welding point. A stainless steel sheath is covered on the outer surface of the heat shrink tube wrapped section. The mouth of the sleeve is connected to a handle so that the stainless steel sheath is located in the inner cavity of the handle. The armored thermocouple and the stainless steel sheath are fixed in the handle cavity by filling with insulating glue. The insulating glue is used to ensure the insulation of the welding point. The stainless steel sheath is used to tighten and support each welding point to improve the stability of the temperature sensor when working. The compensation wire is wrapped with a heat shrink tube, and extends out of the handle to connect the connectors.

[0015] Furthermore, when the armored thermocouple is a K-type thermocouple, the insulating glue is epoxy resin.

[0016] Furthermore, when the armored thermocouple is an S-type thermocouple, the insulating glue is a high-temperature resistant inorganic glue, and the high-temperature resistant inorganic glue is a commercially available C-2 inorganic glue.

[0017] Furthermore, the materials of the outer wall of the compensation wire are polyvinyl chloride, glass wire braided sheath, stainless steel wire braided shielding wire, and polyvinyl chloride from the inside to the outside, which plays a good role in electrical insulation, shielding, and corrosion resistance for the cold end of the armored thermocouple.

[0018] Furthermore, the sleeve is a quartz sleeve. The quartz material has the characteristics of high temperature resistance and corrosion resistance. The hydroxyl content of the quartz sleeve is ≤220ppm. The hydroxyl content is small. The quartz sleeve is not easy to crystallize at high temperature, thereby improving the service life of the thermocouple.

[0019] Furthermore, the handle is made of stainless steel, which is strong, high temperature resistant and corrosion resistant.

[0020] The functions of each element in the material of the present invention are as follows:

[0021] Lanthanum: It is a metallic rare earth element that can form an oxide film on the surface of the wire. Lanthanum oxide is distributed on the surface of the wire to avoid phosphorus and boron contamination of the wire in the corrosive environment of phosphorus and boron in the diffusion furnace, which can induce intergranular corrosion and breakage of the wire at high temperature.

[0022] Gadolinium: It is a metallic rare earth element. The main strengthening mechanism of trace amounts of gadolinium on the alloy is second phase strengthening and solid solution strengthening. During the production process of the twin wire, fine gadolinium oxide particles are formed and pinned between the grains, which strengthens the connection between the grains and reduces the impact of intergranular corrosion caused by phosphorus diffusion and boron diffusion.

[0023] Scandium: The chemical properties of scandium are stable, and it is easy to form an impermeable passivation layer on the surface of the dual wire, avoiding the corrosion of phosphorus and boron on the dual wire. At the same time, in the environment of photovoltaic phosphorus diffusion and boron diffusion furnace, it has excellent stability and corrosion resistance, and can resist the corrosion of phosphorus and boron.

[0024] Nickel-chromium alloy (NiCr10 alloy):

[0025] Strength and toughness under high temperature service: NiCr10 nickel-chromium alloy can maintain high strength and toughness at high temperatures, so it has excellent durability when used in high temperature environments.

[0026] High temperature oxidation resistance: NiCr10 nickel-chromium alloy is not easy to rust or corrode in high temperature, high pressure and strong oxidation environment, so it has a longer service life in oxidizing environment.

[0027] Nickel silicon alloy (NiSi3 alloy):

[0028] Toughness: NiSi3 alloy has high strength and hardness, but its toughness is still well maintained.

[0029] Corrosion resistance: NiSi3 alloy has good corrosion resistance and can maintain its original performance and life in a variety of corrosive media.

[0030] Platinum (Pt): It has extremely stable chemical properties, is insoluble in strong acids and alkalis, and is not easily oxidized in the air.

[0031] Platinum-rhodium 10 alloy (PtRh10 alloy): has strong corrosion resistance, rhodium can improve the alloy's oxidation resistance and acid corrosion resistance. When heated in a high-temperature oxidizing atmosphere, rhodium can reduce the volatilization loss of platinum in the alloy.

[0032] The technical effects of the present invention are:

[0033] (1) Compared with the prior art, the K-type and S-type armored thermocouples of the integrated multi-point temperature sensor of the present invention have three components added, namely lanthanum, gadolinium and scandium, which improves the corrosion resistance of the integrated multi-point temperature sensor.

[0034] (2) Compared with ordinary assembled thermocouples, the armored thermocouple of the present invention has better mechanical properties, high temperature erosion resistance, high temperature corrosion resistance and corrosion resistance, which greatly improves the service stability and service life of the integrated multi-point temperature sensor.

[0035] (3) The integrated multi-point temperature sensor of the present invention can measure multiple temperature points simultaneously in the environment of a photovoltaic phosphorus diffusion furnace or a photovoltaic boron diffusion furnace, and has high temperature measurement accuracy and long service life.

[0036] (4) The applicant's experiments show that: the accuracy test results of the K-type wire couple meet the requirements of Class I accuracy of GB / T 2614-2010, the results of the mechanical property test of the K-type wire couple meet the requirements of GB / T 1234-2012, and the results of the corrosion resistance test of the K-type wire couple meet the requirements of GB / T 4334-2020 for intergranular corrosion performance; the accuracy test results of the S-type wire couple meet the requirements of Class I accuracy of GB / T 1598-2010, the results of the mechanical property test of the S-type wire couple meet the requirements of GB / T 1598-2010, and the results of the corrosion resistance test of the S-type wire couple meet the requirements of GB / T 4334-2020 for intergranular corrosion performance; therefore, the wire couples of the K-type and S-type armored thermocouples and the integrated multi-point temperature sensor prepared from the material of the present invention have excellent service stability. In the complex atmosphere environment of the crystalline silicon growth diffusion furnace used in the photovoltaic field, the service life is greater than 10 months at a long-term working temperature of 1050°C, which greatly improves the service life. The integrated multi-point temperature sensor made of different K-type or S-type thermocouple wires is used in different working environments. The sensor is highly integrated and has the advantages of good temperature measurement stability, high measurement accuracy, good corrosion resistance and easy installation. The maximum operating temperature can reach 1300℃ and can also be promoted to temperature measurement and control in other high-temperature industrial fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a structural schematic diagram of the present invention.

[0038] Figure 2 for Figure 1 Enlarged view of point A in the middle.

[0039] Description of the reference numerals: sleeve 1, armored thermocouple 2, thermocouple wire 3, compensation wire 4, heat shrink tube 5, stainless steel sheath 6, handle 7, insulating glue 8, connector 9. DETAILED DESCRIPTION

[0040] Table 1 Weight parts of each component used to prepare the K-type thermocouple wire

[0041]

[0042] Table 2 Weight parts of each component used to prepare S-type thermocouple wire

[0043]

[0044] Embodiment 7

[0045] This embodiment is a method for preparing the K-type thermocouple wires in the preparation of embodiments 1 to 3.

[0046] High-purity nickel, chromium, and silicon (purity ≥ 99.99%) are used as raw materials. Nickel, chromium, lanthanum, gadolinium, and scandium are weighed as positive electrodes according to weight, and nickel, silicon, lanthanum, gadolinium, and scandium are weighed as negative electrodes according to weight. The ingredients are weighed separately and loaded into a crucible, and then placed in a vacuum induction melting furnace to be melted into ingots (nickel-chromium alloy ingots and nickel-silicon alloy ingots, respectively). After the ingots are finished, they are placed in a heating furnace for heat treatment. The heating temperature of the nickel-chromium alloy ingot is 900℃~1100℃, and the heating temperature of the nickel-silicon alloy ingot is 800℃~1000℃, and the heat preservation is carried out for 30~50min. The ingots are forged into square bars with a cross-sectional size of 10mm×10mm. The annealing temperature after forging is 800℃~1100℃, and the heat preservation is carried out for 20~30min. The forged bars are rolled, and the pass processing rate is controlled at 15~20%, and finally rolled into The round bar is annealed at 800℃~1100℃ and kept warm for 20~30min. Then the nickel-chromium alloy bar and the nickel-silicon alloy bar are drawn through the wire drawing die. Pull into The nickel-chromium alloy wire and nickel-silicon alloy wire are processed at a rate of 15-20%. The wire is cleaned and then continuously annealed before being rewound at a temperature of 800°C to 1100°C. The positive and negative wires are cut and welded in pairs according to different lengths, and armor technology is used to form an integrated armored thermocouple.

[0047] Embodiment 8

[0048] This embodiment is a method for preparing the S-type thermocouple wires in the fourth to sixth embodiments.

[0049] Sponge platinum (purity ≥ 99.99%) and high-purity rhodium powder (purity ≥ 99.95%) are used as raw materials. Platinum, rhodium, lanthanum, gadolinium and scandium are weighed as positive electrodes according to their weight proportions, and platinum, lanthanum, gadolinium and scandium are weighed as negative electrodes according to their weight proportions. The ingredients are weighed separately and loaded into a crucible for induction heating and smelting into ingots (platinum ingots and platinum-rhodium 10 alloy ingots, respectively). After finishing, the ingots are placed in a heating furnace for heat treatment. The heating temperature of the platinum ingot is 600℃~800℃, and the heating temperature of the platinum-rhodium 10 alloy ingot is 1200℃~1300℃, and the heat preservation is carried out for 15~20min. The ingots are forged into square bars with a cross-sectional size of 10mm×10mm. The annealing temperature after forging is 700℃~1300℃, and the heat preservation is carried out for 15~20min. The forged bars are rolled, and the pass processing rate is controlled at 7~10%, and finally rolled into The round bar is annealed at 700℃~1300℃ and kept warm for 15~20min. Then the platinum bar and platinum-rhodium 10 alloy bar are drawn through the wire drawing die. Pull into The platinum wire and platinum-rhodium 10 alloy wire are processed at a rate of 15-20%. The wire is cleaned and then continuously annealed and rewound at a temperature of 700°C to 1300°C. The positive and negative electrode wires are cut according to different lengths and welded in pairs.

[0050] Embodiment 9

[0051] This embodiment takes 7 temperature measurement points as an example to describe the method for making an integrated multi-point temperature sensor. The integrated multi-point temperature sensor uses the K-type wire prepared in Example 7. The integrated multi-point temperature sensor is suitable for a photovoltaic phosphorus diffusion furnace.

[0052] The K-type thermocouple wire 3 with a wire diameter of φ0.5 mm prepared in Example 7 is selected, and the positive and negative electrodes of the 7 pairs of thermocouple wires 3 are cut into 800 mm, 1600 mm, 2400 mm, 3200 mm, 3600 mm, 3720 mm, and 3850 mm respectively according to the required length of the temperature measurement point, which is suitable for different temperature zones. The φ0.5 mm K-type thermocouple wire 3 is installed on a sintered φ3.0 mm alumina insulating porcelain column, and then installed together in a φ3.5 mm GH3039 sleeve, and is formed into a K-type thermocouple armor material after one drawing. According to the GB / T2614-2010 standard, the thermoelectric performance of the thermocouple wire 3 is tested (including thermoelectromotive force and tolerance) at four temperature measurement points of 400°C, 600°C, 800°C, and 1000°C. The results of the accuracy test meet the requirements of GB / T 2614-2010 and reach Class I accuracy, as shown in Table 3. According to GB / T1234-2012 standard, the tensile strength, yield strength and elongation after fracture of the dual wire 3 were tested, and the results of the mechanical properties test met the requirements of GB / T 1234-2012, as shown in Table 4. The corrosion resistance of the dual wire 3 was tested in the environment of phosphorus oxychloride and trimethyl borate, and the results of the corrosion resistance test met the requirements of GB / T 4334-2020 for intergranular corrosion performance, as shown in Table 5.

[0053] Table 3: Thermoelectric performance test results

[0054]

[0055] Table 4: Mechanical properties test results

[0056] performance Tensile strength(MPa) Yield strength (MPa) Elongation after break (%) Nichrome 894 673 11.3 Nickel Silicon Alloy 752 543 14.5

[0057] Table 5: Corrosion resistance test results

[0058] temperature Corrosive environment Corrosion time Bending Angle Test results 1000℃ Phosphorus oxychloride 200h Bend 180° No cracks caused by intergranular corrosion 1000℃ Trimethyl borate 200h Bend 180° No cracks caused by intergranular corrosion

[0059] The compensation conductor 4 uses a K-type compensation conductor. The materials of the outer wall of the compensation conductor 4 are polyvinyl chloride, glass fiber braided sheath, stainless steel wire braided shielded wire, and polyvinyl chloride from the inside to the outside, which plays a good role in electrical insulation, shielding, and corrosion resistance for the cold end of the armored thermocouple 2. The length of the compensation conductor 4 is 1000mm. The two ends of the K-type compensation conductor are stripped, and one end is welded to the positive and negative poles of the couple wire 3. A high-power handheld laser welder is used for welding. The advantage of laser welding is that it is easy to form a good molten weld, and the welding efficiency is high and more precise. After welding, use a heat shrink tube 5 to heat shrink the two ends of the welding point. Heat shrinkage is used to seal the welding point to ensure the insulation and corrosion resistance of the welding point. Then use a length of The stainless steel sheath 6 is fixed to the welding point by glue (epoxy resin), the insulating glue 8 is used to ensure the insulation of the welding point, and the stainless steel sheath 6 is used to fasten and support each welding point to improve the stability of the temperature sensor during operation. The resistance value of the positive and negative electrodes of the 7 armored thermocouples 2 is measured by a multimeter, and the resistance value range is 6.2~59.2Ω. The positive and negative electrodes of the armored thermocouples 2 are conductive; and when the heating and cooling rate reaches 20℃ / min, the armored thermocouples 2 do not break.

[0060] The cold ends of the 7 welded armored thermocouples 2 of different lengths are bundled and fixed with nickel-chromium wires. The advantages of nickel-chromium wires are that they do not deform in high temperature environments and have high strength. The sleeve 1 uses a transparent quartz sleeve for photovoltaic semiconductors. The 7 bundled and fixed armored thermocouples 2 are placed in the quartz sleeve. The mouth of the quartz sleeve is fixedly connected to the handle 7. The handle 7 is made of stainless steel. The stainless steel material is strong, resistant to high temperature and corrosion. The armored thermocouple 2 is clamped and fixed in the handle 7 with a ferrule. The compensation wire 4 is heat-shrunk into a bundle with a heat shrink tube 5 and passed through the handle 7. The positive and negative poles of the compensation wire 4 are connected with a K-graded connector 9. The integrated multi-point temperature sensor is completed.

[0061] Embodiment 10

[0062] This embodiment takes 6 temperature measurement points as an example to describe the method for making an integrated multi-point temperature sensor. The integrated multi-point temperature sensor uses the S-type wire prepared in Example 8. The integrated multi-point temperature sensor is suitable for a photovoltaic boron diffusion furnace.

[0063] The S-type dual wire with a wire diameter of 0.35 mm prepared in Example 8 was selected, and according to the required length of the temperature measuring point, the positive and negative electrodes of the 6 pairs of dual wires 3 were cut and welded in pairs according to the lengths of 650 mm, 1400 mm, 2200 mm, 2500 mm, 3000 mm and 3550 mm respectively. According to GB / T 1598-2010, the thermoelectric performance test (including thermoelectromotive force and tolerance) of the dual wire 3 was carried out at three temperature measurement points of 419.527℃, 660.323℃ and 1084.62℃. The results of the precision test met the requirements of GB / T 1598-2010 and achieved Class I precision, as shown in Table 6; the mechanical properties of tensile strength, yield strength and elongation after fracture were tested on the dual wire 3 according to GB / T 1598-2010. The results of the mechanical properties test met the requirements of GB / T 1598-2010, as shown in Table 7; the corrosion resistance test of the dual wire 3 in the environment of phosphorus oxychloride and trimethyl borate was carried out. The results of the corrosion resistance test met the requirements of intergranular corrosion performance of GB / T4334-2020, as shown in Table 8.

[0064] Table 6: Test results of thermoelectric performance of coupled wires

[0065]

[0066] Table 7: Test results of mechanical properties of even wire

[0067] Tensile strength(MPa) Yield strength (MPa) Elongation after break (%) Platinum-Rhodium Alloy 327 174 25.3 Doped platinum 156 28 39.2

[0068] Table 8: Test results of corrosion resistance of even wire

[0069] temperature Corrosive environment Corrosion time Bending Angle Test results 1084℃ Phosphorus oxychloride 200h Bend 180° No cracks caused by intergranular corrosion 1084℃ Trimethyl borate 200h Bend 180° No cracks caused by intergranular corrosion

[0070] A high-purity corundum double-hole ceramic core that is extruded and sintered is selected as the insulating carrier of the dual wire 3. The purity of the high-purity corundum double-hole ceramic core is more than 99.9%, and the purity is high, which can avoid the contamination of the dual wire 3 by impurities at high temperature. The lengths of the 6 high-purity corundum double-hole ceramic cores are 630mm, 1380mm, 2180mm, 2580mm, 2980mm, and 3530mm respectively. The corundum double-hole ceramic core is ventilated with compressed air to blow out the impurities in the double holes to ensure the smooth flow of the corundum double-hole ceramic core. Then, it is calcined at 1200℃ for 16h. The calcination is conducive to the volatilization of impurities, avoiding the contamination of the dual wire 3 by impurities at high temperature, reducing the problem of inaccurate temperature measurement and breakage of the dual wire 3 caused by impurity contamination, and improving the service life of the integrated multi-point temperature sensor. The wound dual wire 3 is straightened with white gauze to avoid bending and winding of the dual wire 3. Finally, the 6 pairs of dual wires 3 are respectively inserted into the corundum double-hole ceramic core to make the thermocouple have good insulation. The resistance value of the positive and negative electrodes of the armored thermocouple 2 was measured with a multimeter, and the resistance value range was 2.3 to 14.0Ω; the positive and negative electrodes of the thermocouple were conductive. When the heating and cooling rate reached 25℃ / min, the thermocouple did not break.

[0071] The compensation wire 4 uses an S-type compensation wire. The materials of the outer wall of the compensation wire 4 are polyvinyl chloride, glass fiber braided sheath, stainless steel wire braided shielded wire, and polyvinyl chloride from the inside to the outside, respectively, which plays a good role in electrical insulation, shielding, and corrosion resistance for the cold end of the armored thermocouple 2. The length of the compensation wire 4 is 1000mm. The ends of the compensation wire 4 are stripped, and the stripping lengths of the two ends are 5mm and 10mm respectively. The 5mm end is welded to the positive and negative poles of the thermocouple wire 3 using a high-power handheld laser welder. The advantage of laser welding is that it is easy to form a good molten weld, with high welding efficiency and more precision. After welding, the heat shrink tube 5 is used to heat shrink the two ends of the welding point as a whole. Heat shrinkage is used to seal the welding point to ensure the insulation and corrosion resistance of the welding point.

[0072] The welding point of the cold end and the high-purity corundum double-hole ceramic core are wrapped and fixed as a whole with a 10mm wide high-temperature insulating glue to improve the insulation and prevent the armored thermocouple 2 from shifting. Then, 6 thermocouples of different lengths are bundled and fixed with a 0.3mm platinum wire and inserted into the sleeve 1. The sleeve 1 is a transparent quartz sleeve for photovoltaic semiconductors. The advantages of platinum wire are high temperature resistance and high strength. The mouth of the quartz sleeve is fixedly connected to the handle 7. The handle 7 is made of stainless steel. The stainless steel material is strong, high temperature resistant and corrosion resistant. The compensation wire 4 is shrunk into a bundle with a heat shrink tube 5 and passed through the handle 7. The welding point is located in the middle of the handle 7. Finally, it is fixed with glue (high temperature resistant inorganic glue, which is commercially available C-2 inorganic glue). After the inorganic glue solidifies, the positive and negative poles of the compensation wire 4 are connected with an S-graded connector 9, and the integrated multi-point temperature sensor is completed.

[0073] The integrated multi-point temperature sensor of the present invention can realize multi-point temperature measurement, has a wide temperature measurement range, is resistant to high temperatures, has high stability, high precision, is corrosion-resistant, has a long service life, has low cost, and is highly applicable.

[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification made to the present invention by those skilled in the art without departing from the spirit of the present invention shall fall within the protection scope of the present invention.

Claims

1. The material used for the integrated multi-point temperature sensor wire pair is characterized by: The wire pair includes a wire pair of a K-type thermocouple or a wire pair of an S-type thermocouple; the weight parts of the components in the positive electrode of the wire pair of the K-type thermocouple are 89.9-90.1 parts of nickel, 9.9-10.1 parts of chromium, 0.001-0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.003 parts of scandium; the weight parts of the components in the negative electrode of the wire pair of the K-type thermocouple are 96.9-97.1 parts of nickel, 2.9-3.1 parts of silicon, 0.001-0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.003 parts of scandium; The weight parts of the components in the positive electrode of the S-type thermocouple are: 89.9-90.1 parts of platinum, 9.9-10.10 parts of rhodium, 0.001-0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.003 parts of scandium. The weight parts of the components in the negative electrode of the S-type thermocouple are: 99.9-100 parts of platinum, 0.001-0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.003 parts of scandium.

2. The material according to claim 1, characterized in that: The weight parts of the components in the positive electrode of the K-type thermocouple are 89.950-89.971 parts of nickel, 10.020-10.040 parts of chromium, 0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.002 parts of scandium; the weight parts of the components in the negative electrode of the K-type thermocouple are 96.930-96.970 parts of nickel, 3.020-3.056 parts of silicon, 0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.002 parts of scandium.

3. The material according to claim 1, characterized in that: The weight proportions of the components in the positive electrode of the S-type thermocouple are 89.950-89.997 parts of platinum, 9.995-10.043 parts of rhodium, 0.003 parts of lanthanum, 0.001-0.002 parts of gadolinium, and 0.001-0.003 parts of scandium; the weight proportions of the components in the negative electrode of the S-type thermocouple are 99.992-99.995 parts of platinum, 0.003 parts of lanthanum, 0.001-0.002 parts of gadolinium, and 0.001-0.003 parts of scandium.

4. An integrated multi-point temperature sensor prepared using the material of claim 1, comprising a sleeve (1) with one end sealed, and a plurality of armored thermocouples (2) of different lengths, wherein the hot ends of the plurality of armored thermocouples (2) of different lengths are inserted into the sleeve (1) to form a plurality of temperature measurement points, characterized in that: The armored thermocouple (2) is a K-type thermocouple or an S-type thermocouple; the thermocouple wire (3) of the S-type thermocouple is inserted into a calcined corundum double-hole ceramic core; The cold end of the armored thermocouple (2) extends out of the outer end of the sleeve (1), and the wires (3) of the armored thermocouple (2) extend out of the cold end and are respectively welded to the compensation wires (4). Each welding point is wrapped with a heat shrink tube (5), and a stainless steel sheath (6) is covered on the outer surface of the wrapped section of the heat shrink tube (5). The outer end of the sleeve (1) is connected to a handle (7), so that the stainless steel sheath (6) is located in the inner cavity of the handle (7). The armored thermocouple (2) and the stainless steel sheath (6) are fixed in the cavity of the handle (7) by filling insulating glue (8). The compensation wires (4) are wrapped with the heat shrink tube (5), extend out of the handle (7) and are respectively connected to the connectors (9); The weight parts of the components in the positive electrode of the K-type thermocouple wire (3) are: 89.9-90.1 parts of nickel, 9.9-10.1 parts of chromium, 0.001-0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.003 parts of scandium; the weight parts of the components in the negative electrode of the K-type thermocouple wire (3) are: 96.9-97.1 parts of nickel, 2.9-3.1 parts of silicon, 0.001-0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.003 parts of scandium; The weight proportions of the components in the positive electrode of the S-type thermocouple wire (3) are: 89.9-90.1 parts of platinum, 9.9-10.10 parts of rhodium, 0.001-0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.003 parts of scandium. The weight proportions of the components in the negative electrode of the S-type thermocouple wire (3) are: 99.9-100 parts of platinum, 0.001-0.003 parts of lanthanum, 0.001-0.003 parts of gadolinium, and 0.001-0.003 parts of scandium.

5. The sensor according to claim 4, characterized in that: The corundum double-hole ceramic core serves as an insulating carrier of the even wire (3).

6. The sensor according to claim 4, characterized in that: When the armored thermocouple (2) is a K-type thermocouple, the insulating glue (8) is epoxy resin.

7. The sensor according to claim 4, characterized in that: When the armored thermocouple (2) is an S-type thermocouple, the insulating glue (8) is a high-temperature resistant inorganic glue.

8. The sensor according to claim 4, characterized in that: The materials of the outer wall of the compensation conductor (4) are, from the inside to the outside, polyvinyl chloride, glass wire braided sheath, stainless steel wire braided shielding wire, and polyvinyl chloride.

9. The sensor according to claim 4, characterized in that: The sleeve (1) is a quartz sleeve.