A bipolar all-solid-state battery and a method for preparing the same

By compounding silver foil or tin foil on the surface of the carbon layer and coating it with a polymer electrolyte, the silver carbon or tin carbon negative electrode is prepared, which solves the problems of internal short circuit risk and high cost of nanosilver materials in bipolar solid-state batteries, and achieves high energy density and Improved safety, suitable for large-scale production.

CN118281360BActive Publication Date: 2024-10-01GUOLIAN CORE MATERIALS (BEIJING) TECHNOLOGY CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202410704048.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-01
Estimated Expiration
2044-06-03

AI Technical Summary

Technical Problem

Existing bipolar solid-state batteries have the risk of internal short circuits during the structural design and manufacturing process, and the preparation cost of nanosilver materials is high, making them unsuitable for use in bipolar solid-state batteries.

Method used

Silver foil or tin foil is directly compounded on the surface of the carbon layer, and a polymer electrolyte coating is coated on the silver foil or tin foil to prepare a silver carbon or tin carbon negative electrode to form a conductive network structure, simplify the process and reduce the amount of metal.

Benefits of technology

It improves the energy density and safety of the battery, reduces the cost, is suitable for large-scale production, avoids the generation of lithium dendrites, and simplifies the process difficulty.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118281360B_ABST
    Figure CN118281360B_ABST
Patent Text Reader

Abstract

The present invention provides a bipolar all-solid-state battery and a preparation method thereof, belonging to the technical field of all-solid-state batteries. Its structural composition is: A(B) n C, A unit includes a stacked current collector and a positive electrode layer, B unit includes a stacked inorganic solid electrolyte layer, a negative electrode layer, a current collector and a positive electrode layer, and C unit includes a stacked inorganic solid electrolyte layer, a negative electrode layer and a current collector; wherein the negative electrode layer includes a conductive carbon layer and a silver foil and / or tin foil composited on the conductive carbon layer, and a polymer electrolyte coating is also provided on the silver foil and / or tin foil. The negative electrode is directly composited with a carbon-coated conductive layer on the silver foil / tin foil, which simplifies the process difficulty, reduces the amount of metal used, and improves the electrical performance of the negative electrode and the entire battery; the polymer electrolyte layer coated on the surface of the silver foil / tin foil is not only conducive to inducing lithium metal deposition, but also plays an electronic insulating role to avoid the formation of lithium dendrites.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of all-solid-state batteries, and specifically relates to a bipolar all-solid-state battery and a preparation method thereof. Background Art

[0002] Energy shortage and environmental pollution are two major problems that the world is concerned about today. Considering the energy supply and exhaust pollution problems brought by traditional cars, the development of new energy vehicles has become an important demand of countries around the world, and the comprehensive replacement of traditional fuel vehicles by new energy vehicles has been put on the agenda. If new energy vehicles want to continue to compete with traditional fuel vehicles in the market, they must be comparable to fuel vehicles in terms of mileage and cost. This requires the energy density of battery cells to reach 350Wh / kg, or even higher. With the increase in the energy density of single cells, its safety risks are also gradually increasing. How to improve the safety of power batteries will become a key focus in the industry. Solid-state batteries using solid electrolytes can reduce or even eliminate the use of liquid electrolytes. In theory, they can effectively reduce the probability of safety accidents such as fire and explosion. They are believed to be able to solve the safety problems of new energy vehicles from the root and become a key development direction in the field of power batteries. At the same time, due to the non-flowing characteristics of solid electrolytes, battery internal series (i.e., bipolar structure) becomes possible, and bipolar structure has also become another important technical approach for solid-state batteries to improve specific energy.

[0003] At present, most of the research on bipolar solid-state batteries is focused on the structural design of bipolar batteries. The patent with publication number CN107180995A provides a bipolar stacked all-solid-state lithium secondary battery and its manufacturing method, and introduces a solid-state battery with a structure that prevents internal short circuits and enables the bipolar stack to be sintered as a whole. The patent with publication number CN116325282A provides a bipolar solid-state battery including a porous support layer, and an insulating porous support layer is arranged between unit cells connected in series with each other. The patent with publication number CN114447263A provides a bipolar solid-state battery with an insulating compression pad, and the compression pad is arranged on the inner side of the inward folded structure of the collector. The above patents mainly focus on the structural design of bipolar solid-state batteries, especially preventing internal short circuits during the assembly process of bipolar solid-state batteries.

[0004] At present, the silver-carbon negative electrode basically focuses on the blending of nanosilver (nanosilver particles or nanosilver wires) with carbon materials. Nanosilver is either generated in situ through a silver precursor or directly blended. The patent with publication number CN107093710A generates a silver-carbon double coating layer by in-situ reduction of a silver ammonia solution on the surface of a carbon-based material. The carbon-based material is coated with a silver-carbon double conductive network layer, with nanoparticle metallic silver as nodes and amorphous carbon as a connection to form a network conductive structure. The patent with publication number CN104577062A first prepares nanosilver sol, and then mixes it with carbon material to prepare silver-carbon negative electrode material for use in lithium-ion batteries. The above-mentioned silver-carbon negative electrode technology has complex nanosilver dispersion, pollution in nanosilver reduction, and high manufacturing process cost, which is not suitable for use in bipolar solid-state batteries. Summary of the invention

[0005] To solve at least one of the problems of the prior art, the present invention provides a bipolar all-solid-state battery, whose negative electrode is a silver foil or a tin foil directly compounded on the surface of a carbon layer to prepare a silver-carbon negative electrode or a tin-carbon negative electrode, and a polymer electrolyte coating is further coated on the silver foil or the tin foil.

[0006] One of the objects of the present invention is to provide a bipolar all-solid-state battery.

[0007] A second object of the present invention is to provide a method for preparing the bipolar all-solid-state battery.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] In a first aspect, the present invention provides a bipolar all-solid-state battery, comprising an A unit, a B unit and a C unit, and the structure thereof is as follows: A(B) n C, n is the number of repetitions of the B unit, and n is an integer from 1 to 100;

[0010] Unit A includes a current collector and a positive electrode layer arranged in layers, unit B includes an inorganic solid electrolyte layer, a negative electrode layer, a current collector and a positive electrode layer arranged in layers, and unit C includes an inorganic solid electrolyte layer, a negative electrode layer and a current collector arranged in layers; the positive electrode layer of one unit B in any two adjacent groups of units B abuts against the inorganic solid electrolyte layer of the other unit B, the positive electrode layer of unit A abuts against the inorganic solid electrolyte layer outside unit B, and the inorganic solid electrolyte layer of unit C abuts against the positive electrode layer outside unit B;

[0011] The negative electrode layer includes a conductive carbon layer and silver foil and / or tin foil composited on the conductive carbon layer. The silver foil and / or tin foil is also provided with a polymer electrolyte coating. The polymer electrolyte coating of the negative electrode layer abuts against the inorganic solid electrolyte layer.

[0012] The layer structures in unit A, unit B and unit C are described in detail below:

[0013] Current collector:

[0014] In some embodiments, the current collector is one selected from stainless steel foil, nickel foil and alloys thereof;

[0015] In some embodiments, the current collector has a thickness of 2 to 30 μm.

[0016] Positive electrode layer:

[0017] The positive electrode layer includes the following components by mass percentage: 70-90% of positive electrode active material, 1-3% of conductive agent, 1-3% of binder and 4-28% of sulfide electrolyte.

[0018] In some embodiments, the positive electrode active material is at least one selected from ternary materials, lithium iron phosphate, lithium cobalt oxide, lithium iron manganese phosphate, and lithium-rich manganese-based materials.

[0019] In some embodiments, the conductive agent is at least one selected from acetylene black, Super P, Super S, 350G, carbon fiber VGCF, carbon nanotubes CNTs, Ketjen black, graphite conductive agent (such as KS-6, KS-15, SFG-6, SFG-15) and graphene.

[0020] In some embodiments, the binder is at least one selected from polyvinylidene fluoride PVDF and modified materials thereof, polytetrafluoroethylene PTFE and modified materials thereof, polyethylene oxide PEO, polypropylene carbonate PPC, polyethylene carbonate PEC, polytrimethylene carbonate PTMC, polyvinyl alcohol PVA, sodium carboxymethyl cellulose CMC, polyolefins (polyethylene, polypropylene and copolymers thereof), hydrogenated styrene-butadiene block copolymer SEBS, cyano rubber NBR, modified SBR, fluorinated rubber, and polyurethane.

[0021] In some embodiments, the sulfide electrolyte is at least one selected from a binary sulfide electrolyte, a ternary sulfide electrolyte, and an argyrodite-type sulfide electrolyte, preferably lithium phosphorus sulfur chloride (Li6PS5Cl).

[0022] In some embodiments, the thickness of the positive electrode layer is 30-150 μm.

[0023] Negative layer:

[0024] The negative electrode layer of the invention comprises a conductive carbon layer and a silver foil and / or a tin foil compounded on the conductive carbon layer, and a polymer electrolyte coating is also arranged on the silver foil and / or the tin foil.

[0025] In some embodiments, the conductive carbon layer includes the following components by mass percentage: 60-90% conductive carbon, 0.5-5% binder, and 5-39.5% sulfide electrolyte.

[0026] In some embodiments, the conductive carbon is at least one selected from conductive carbon black, carbon nanotubes, graphene, fullerene, and carbon nanofibers.

[0027] In some embodiments, the binder is at least one selected from polyvinylidene fluoride PVDF and modified materials thereof, polytetrafluoroethylene PTFE and modified materials thereof, polyethylene oxide PEO, polypropylene carbonate PPC, polyethylene carbonate PEC, polytrimethylene carbonate PTMC, polyvinyl alcohol PVA, sodium carboxymethyl cellulose CMC, polyolefins (polyethylene, polypropylene and copolymers thereof), hydrogenated styrene-butadiene block copolymer SEBS, cyano rubber NBR, modified SBR, fluorinated rubber, and polyurethane.

[0028] In some embodiments, the sulfide electrolyte is at least one selected from a binary sulfide electrolyte, a ternary sulfide electrolyte, and an argyrodite-type sulfide electrolyte, preferably lithium phosphorus sulfur chloride (Li6PS5Cl).

[0029] In some embodiments, the conductive carbon layer has a thickness of 0.5-10 μm.

[0030] In some embodiments, the thickness of the silver foil is 0.1-2 μm, and the thickness of the tin foil is 0.5-10 μm.

[0031] In some embodiments, the polymer electrolyte coating includes polyethylene oxide (PEO) or its modified material, lithium salt and inorganic particles; the molar ratio of ether bonds to lithium salt in PEO or its modified material is 17 to 20:1, preferably 18:1; the mass of the inorganic particles is 10 to 50% of the total mass of the lithium salt and PEO or its modified material.

[0032] In some embodiments, the molecular weight of PEO or its modified material is 450,000 to 4.5 million;

[0033] In some embodiments, the lithium salt is at least one selected from lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium bis(difluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), and lithium difluorooxalatoborate (LiDFOB);

[0034] In some embodiments, the inorganic particles are at least one selected from lithium aluminum titanium phosphate (LATP), alumina, boehmite, and silica.

[0035] In some embodiments, the thickness of the polymer electrolyte coating is 0.1-5 μm.

[0036] In some embodiments, the length and width of the positive electrode layer are L1 and L2 respectively, and the length and width of the current collector, the negative electrode layer and the inorganic solid electrolyte layer are L'1 and L'2 respectively, and the size relationship is 0.2mm≤L'1-L1≤3mm, 0.2mm≤L'2-L2≤3mm.

[0037] Inorganic solid electrolyte layer:

[0038] In some embodiments, the inorganic solid electrolyte layer is at least one selected from a sulfide electrolyte and an oxide electrolyte; preferably lithium phosphorus sulfur chloride (Li6PS5Cl).

[0039] In some embodiments, the thickness of the inorganic solid electrolyte layer is 5 to 100 μm.

[0040] It should be noted that the negative electrode layer, current collector, positive electrode layer and solid electrolyte described in unit A, unit B and unit C generally refer to the same negative electrode layer, current collector, positive electrode layer and solid electrolyte.

[0041] In a second aspect, the present invention provides a method for preparing the above-mentioned bipolar all-solid-state battery, comprising the following steps:

[0042] Preparation of A unit: a positive electrode layer is arranged on one side of the current collector to form an A unit;

[0043] Preparation of C unit: a conductive carbon layer, a silver foil and / or a tin foil, and a polymer electrolyte coating are sequentially arranged on one side of the current collector to form a negative electrode layer, and an inorganic solid electrolyte layer is then arranged on the polymer electrolyte coating to form a C unit;

[0044] Preparation of unit B: a positive electrode layer is arranged on one side of the current collector, a conductive carbon layer, a silver foil and / or a tin foil, and a polymer electrolyte coating are arranged in sequence on the other side of the current collector to form a negative electrode layer, and an inorganic solid electrolyte layer is arranged on the polymer electrolyte coating to form unit B;

[0045] The A unit, n groups of B units and C units are stacked in order, with the current collectors of the A unit and the C unit facing outward, and the inside is arranged in the order of positive electrode layer, inorganic solid electrolyte layer and negative electrode layer, packaged, and isostatically pressed to obtain a bipolar all-solid-state battery.

[0046] Specifically, the preparation method of the bipolar all-solid-state battery comprises the following steps:

[0047] Prepare the positive electrode layer slurry: completely dissolve the binder in a solvent (such as xylene), add the positive electrode active material, conductive agent and sulfide electrolyte and stir well;

[0048] Prepare conductive carbon layer slurry: fully stir conductive carbon, sulfide electrolyte, binder, and solvent (such as xylene);

[0049] Preparation of polymer electrolyte coating slurry: dissolve polyethylene oxide (PEO) or its modified material in a solvent (such as NMP, DMAC, DMF, etc.) to obtain a polymer solution with a solid content of 2%-20%, add lithium salt, fully complex for more than 6 hours, then add inorganic particles and disperse evenly. The solid content of the entire slurry is controlled at 5-40%;

[0050] Prepare the inorganic solid electrolyte layer slurry: mix the sulfide electrolyte into a solution containing 1-10% of a binder (such as a xylene solution of SEBS), stir thoroughly, add xylene, adjust the solid content to 30-70%, and stir thoroughly;

[0051] Preparation of unit A: coating the positive electrode layer slurry on one side of the current collector, drying, cutting into required size, and setting aside;

[0052] Preparation of C unit: coating the conductive carbon layer slurry on one side of the current collector, drying to obtain the conductive carbon layer; compounding the silver foil and / or tin foil on the conductive carbon layer by roller pressing; spinning the polymer electrolyte coating slurry on the surface of the silver foil and / or tin foil by electrostatic spinning equipment, drying to obtain the polymer electrolyte coating; coating the inorganic solid electrolyte layer slurry on the polymer electrolyte coating, drying, cutting into required size, and setting aside;

[0053] Preparation of unit B: coating the positive electrode layer slurry on one side of the current collector and drying; coating the conductive carbon layer slurry on the other side of the current collector and drying to obtain a conductive carbon layer; compounding the silver foil and / or tin foil on the conductive carbon layer by roller pressing; spinning the polymer electrolyte coating slurry on the surface of the silver foil and / or tin foil by electrostatic spinning equipment and drying to obtain a polymer electrolyte coating; coating the inorganic solid electrolyte layer slurry on the polymer electrolyte coating, drying, cutting into required size, and setting aside;

[0054] The A unit, n groups of B units and C units are stacked in order, with the current collectors of the A unit and the C unit facing outwards. The inside is arranged in the order of positive electrode layer, inorganic solid electrolyte layer and negative electrode layer. After arrangement, they are packaged with aluminum-plastic film and isostatically pressed at a pressure of 100~1000MPa to obtain a soft-pack solid-state battery cell.

[0055] Preferably, the specific steps of electrospinning are: adding the polymer electrolyte coating slurry into the syringe of the electrospinning equipment, the needle aperture is 0.5-1.8mm, the spinning voltage is 15-50kV, the receiving distance between the needle and the silver foil and / or tin foil is 16-30cm, and the spinning time is 30min-3h.

[0056] Beneficial effects:

[0057] The all-solid-state battery of the present invention adopts a bipolar structure, which can greatly improve the battery output voltage and enhance the battery energy density, which is beneficial to reduce the assembly auxiliary parts in later applications and improve the assembly efficiency; the negative electrode uses a carbon-coated conductive layer to directly compound the silver foil / tin foil, which simplifies the process difficulty, reduces the metal dosage, and improves the electrical performance of the negative electrode and the entire battery; the polymer electrolyte layer coated on the surface of the silver foil / tin foil is beneficial to inducing lithium metal deposition, and can also play the role of electronic insulation to avoid the formation of lithium dendrites.

[0058] The method of the present invention does not require the preparation of nano silver materials, does not require the silver reduction process, is environmentally friendly and efficient, and is particularly suitable for application in bipolar solid-state batteries. The method has simple process conditions, controllable preparation conditions and costs, and is suitable for large-scale production.

[0059] The present invention has been described in detail above, but the above embodiments are only illustrative in nature and are not intended to limit the present invention. In addition, this article is not limited by any theory described in the above prior art or invention content or the following examples. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 Schematic diagram of the bipolar all-solid-state battery of the present invention.

[0061] Illustration: 1-positive electrode layer; 2-current collector; 3-inorganic solid electrolyte layer; 4-negative electrode layer. DETAILED DESCRIPTION

[0062] The present invention is further described below in conjunction with examples. It should be noted that the following examples are provided for illustrative purposes only and do not constitute a limitation on the scope of protection claimed for the present invention.

[0063] Unless otherwise specified, the raw materials, reagents, methods, etc. used in the examples are conventional raw materials, reagents, methods in the art.

[0064] 811 ternary materials come from Dangsheng Technology;

[0065] SEBS binder was from MacLean Reagents;

[0066] Polyethylene oxide (PEO) was from MacLean Reagent Company;

[0067] Li6PS5Cl is manufactured by Guolian Battery, model SCD-13 (refer to patent CN110085908A).

[0068] The slurry used in the embodiment is as follows:

[0069] Prepare the positive electrode layer slurry: completely dissolve the SEBS binder (dry powder mass fraction 2%) in the solvent xylene, add 811 ternary material (dry powder mass fraction 80%), VGCF (dry powder mass fraction 2%) and Li6PS5Cl (dry powder mass fraction 16%) and stir well to form a stable slurry;

[0070] Prepare conductive carbon layer slurry: fully stir conductive carbon black CNT (mass fraction 60%), Li6PS5Cl (mass fraction 36%), SEBS binder (mass fraction 4%), and solvent xylene to form a uniform and stable slurry;

[0071] Prepare polymer electrolyte coating slurry: dissolve 3g PEO (ether bond 0.06818mol) with a molecular weight of 3 million in 97g DMF to obtain a PEO solution with a solid content of 3%, add 1.09g LiTFSI, stir well for more than 6 hours, add 1g LATP with an average particle size of 300nm, and disperse evenly;

[0072] Prepare the inorganic solid electrolyte layer slurry: mix 98g Li6PS5Cl into 2% binder solution (SEBS xylene solution), stir well, add xylene, adjust the solid content to 45%, and stir well.

[0073] Example

[0074] The structure of a bipolar all-solid-state battery is as follows Figure 1 As shown, the preparation method is as follows:

[0075] Preparation of unit A: Apply the positive electrode layer slurry to one side of the current collector 2 with a coating amount of 18 mg / cm 2 , drying and rolling to form a positive electrode layer 1, and then cutting into required sizes for standby use;

[0076] Preparation of C unit: coating the conductive carbon layer slurry on one side of the current collector 2, drying to obtain a conductive carbon layer; compounding the silver foil (or tin foil) on the conductive carbon layer by roller pressing; spinning the polymer electrolyte coating slurry on the surface of the silver foil (or tin foil) by electrostatic spinning equipment, drying to obtain a polymer electrolyte coating, and forming a negative electrode layer 4; coating the inorganic solid electrolyte layer slurry on the polymer electrolyte coating, drying to form an inorganic solid electrolyte layer 3, cutting into a required size, and setting aside;

[0077] Preparation of unit B: Apply the positive electrode layer slurry to one side of the current collector 2 with a coating amount of 18 mg / cm 2, drying to form a positive electrode layer 1; applying the conductive carbon layer slurry to the other side of the current collector 2, drying to obtain a conductive carbon layer; compounding the silver foil (or tin foil) on the conductive carbon layer by roller pressing; spinning the polymer electrolyte coating slurry on the surface of the silver foil (or tin foil) by an electrostatic spinning device, drying to obtain a polymer electrolyte coating, forming a negative electrode layer 4; applying the inorganic solid electrolyte layer slurry on the polymer electrolyte coating, drying to form an inorganic solid electrolyte layer 3, cutting into a required size for standby use;

[0078] The specific steps of electrospinning are as follows: add the polymer electrolyte coating slurry into the syringe of the electrospinning equipment, the needle aperture is 0.5-1.8mm, the spinning voltage is 15-50kV, the receiving distance between the needle and the silver foil (or tin foil) is 16-30cm, and the spinning time is 30min-3h;

[0079] The A unit, n groups of B units and C units are stacked in order, with the current collectors 2 of the A unit and the C unit facing outwards, and the inside is arranged in the order of the positive electrode layer 1, the inorganic solid electrolyte layer 3, and the negative electrode layer 4. After arrangement, they are packaged with aluminum-plastic film and isostatically pressed at a pressure of 100~1000MPa to obtain a soft-pack solid-state battery cell.

[0080] The specific materials and results of each embodiment and comparative example are shown in the following table.

[0081]

[0082] Note: The preparation of nano-silver and nano-tin coatings in Comparative Examples 1 and 2 refers to CN104577062A.

[0083] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents, without departing from the spirit and essence of the claims of the present invention; and these modifications or replacements are still within the scope defined by the claims of the present invention.

Claims

1. A bipolar all-solid-state battery, characterized in that: The bipolar all-solid-state battery comprises an A unit, a B unit and a C unit, and its structure is as follows: A(B) n C, n is the number of repetitions of the B unit, and n is an integer from 1 to 100; Unit A includes a current collector and a positive electrode layer arranged in layers, unit B includes an inorganic solid electrolyte layer, a negative electrode layer, a current collector and a positive electrode layer arranged in layers, and unit C includes an inorganic solid electrolyte layer, a negative electrode layer and a current collector arranged in layers; the positive electrode layer of one unit B in any two adjacent groups of units B abuts against the inorganic solid electrolyte layer of the other unit B, the positive electrode layer of unit A abuts against the inorganic solid electrolyte layer outside unit B, and the inorganic solid electrolyte layer of unit C abuts against the positive electrode layer outside unit B; The negative electrode layer includes a conductive carbon layer and a silver foil and / or tin foil composited on the conductive carbon layer, the silver foil and / or tin foil is further provided with a polymer electrolyte coating, and the polymer electrolyte coating of the negative electrode layer abuts against the inorganic solid electrolyte layer; The conductive carbon layer comprises the following components by mass percentage: 60-90% conductive carbon, 0.5-5% binder and 5-39.5% sulfide electrolyte; The polymer electrolyte coating includes polyethylene oxide or its modified material, lithium salt and inorganic particles; the molar ratio of ether bond to lithium salt in polyethylene oxide or its modified material is 17-20:1, and the mass of the inorganic particles is 10-50% of the total mass of the lithium salt and polyethylene oxide or its modified material.

2. The bipolar all-solid-state battery according to claim 1, characterized in that: The current collector is one selected from stainless steel foil, nickel foil and alloys thereof; the thickness of the current collector is 2-30 μm.

3. The bipolar all-solid-state battery according to claim 1, characterized in that: The positive electrode layer includes the following components by mass percentage: 70-90% positive electrode active material, 1-3% conductive agent, 1-3% binder and 4-28% sulfide electrolyte; The positive electrode active material is at least one selected from ternary materials, lithium iron phosphate, lithium cobalt oxide, lithium iron manganese phosphate, and lithium-rich manganese-based materials; The conductive agent is at least one selected from acetylene black, Super P, Super S, 350G, carbon fiber VGCF, carbon nanotubes CNTs, Ketjen black, graphite conductive agent, and graphene; The binder is at least one selected from polyvinylidene fluoride PVDF and modified materials thereof, polytetrafluoroethylene PTFE and modified materials thereof, polyethylene oxide PEO, polypropylene carbonate PPC, polyethylene carbonate PEC, polytrimethylene carbonate PTMC, polyvinyl alcohol PVA, sodium carboxymethyl cellulose CMC, polyolefins, hydrogenated styrene-butadiene block copolymer SEBS, cyano rubber NBR, modified SBR, fluorinated rubber, and polyurethane; The sulfide electrolyte is at least one selected from a binary sulfide electrolyte, a ternary sulfide electrolyte and an argyrodite-type sulfide electrolyte; The thickness of the positive electrode layer is 30~150μm.

4. The bipolar all-solid-state battery according to claim 1, characterized in that: The conductive carbon is at least one selected from conductive carbon black, carbon nanotubes, graphene, fullerene, and carbon nanofibers; The binder is at least one selected from polyvinylidene fluoride PVDF and modified materials thereof, polytetrafluoroethylene PTFE and modified materials thereof, polyethylene oxide PEO, polypropylene carbonate PPC, polyethylene carbonate PEC, polytrimethylene carbonate PTMC, polyvinyl alcohol PVA, sodium carboxymethyl cellulose CMC, polyolefins, hydrogenated styrene-butadiene block copolymer SEBS, cyano rubber NBR, modified SBR, fluorinated rubber, and polyurethane; The sulfide electrolyte is at least one selected from a binary sulfide electrolyte, a ternary sulfide electrolyte and an argyrodite-type sulfide electrolyte; The thickness of the conductive carbon layer is 0.5~10μm.

5. The bipolar all-solid-state battery according to claim 1, characterized in that: The thickness of silver foil is 0.1~2μm, and the thickness of tin foil is 0.5~10μm.

6. The bipolar all-solid-state battery according to claim 1, characterized in that: The molecular weight of polyethylene oxide or its modified material is 450,000 to 4.5 million; The lithium salt is at least one selected from lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium bis(difluorosulfonyl imide), lithium bis(trifluoromethylsulfonyl imide), and lithium difluorooxalatoborate; The inorganic particles are at least one selected from lithium aluminum titanium phosphate, aluminum oxide, boehmite, and silicon dioxide; The thickness of the polymer electrolyte coating is 0.1~5μm.

7. The bipolar all-solid-state battery according to claim 1, characterized in that: The inorganic solid electrolyte layer is at least one selected from a sulfide electrolyte and an oxide electrolyte; the thickness of the inorganic solid electrolyte layer is 5 to 100 μm.

8. The bipolar all-solid-state battery according to claim 1, characterized in that: The length and width of the positive electrode layer are L1 and L2 respectively, and the length and width of the current collector, negative electrode layer and inorganic solid electrolyte layer are L'1 and L'2 respectively, and the size relationship is 0.2mm≤L'1-L1≤3mm, 0.2mm≤L'2-L2≤3mm.

9. A method for preparing a bipolar all-solid-state battery according to any one of claims 1 to 8, characterized in that: The following steps are involved: Preparation of A unit: a positive electrode layer is arranged on one side of the current collector to form an A unit; Preparation of C unit: a conductive carbon layer, a silver foil and / or a tin foil, and a polymer electrolyte coating are sequentially arranged on one side of the current collector to form a negative electrode layer, and an inorganic solid electrolyte layer is then arranged on the polymer electrolyte coating to form a C unit; Preparation of unit B: a positive electrode layer is arranged on one side of the current collector, a conductive carbon layer, a silver foil and / or a tin foil, and a polymer electrolyte coating are arranged in sequence on the other side of the current collector to form a negative electrode layer, and an inorganic solid electrolyte layer is arranged on the polymer electrolyte coating to form unit B; The A unit, n groups of B units and C units are stacked in order, with the current collectors of the A unit and the C unit facing outward, and the inside is arranged in the order of positive electrode layer, inorganic solid electrolyte layer and negative electrode layer, packaged, and isostatically pressed to obtain a bipolar all-solid-state battery.

10. The preparation method according to claim 9, characterized in that: The following steps are involved: Preparation of unit A: coating the positive electrode layer slurry on one side of the current collector, drying, cutting into required size, and setting aside; Preparation of C unit: coating the conductive carbon layer slurry on one side of the current collector, drying to obtain the conductive carbon layer; compounding the silver foil and / or tin foil on the conductive carbon layer by roller pressing; spinning the polymer electrolyte coating slurry on the surface of the silver foil and / or tin foil by electrostatic spinning equipment, drying to obtain the polymer electrolyte coating; coating the inorganic solid electrolyte layer slurry on the polymer electrolyte coating, drying, cutting into required size, and setting aside; Preparation of unit B: coating the positive electrode layer slurry on one side of the current collector and drying; The conductive carbon layer slurry is coated on the other side of the current collector and dried to obtain a conductive carbon layer; the silver foil and / or tin foil are compounded on the conductive carbon layer by roller pressing; the polymer electrolyte coating slurry is spun on the surface of the silver foil and / or tin foil by an electrostatic spinning device and dried to obtain a polymer electrolyte coating; the inorganic solid electrolyte layer slurry is coated on the polymer electrolyte coating, dried, and cut into a required size for standby use; The A unit, n groups of B units and C units are stacked in order, with the current collectors of the A unit and the C unit facing outwards. The inside is arranged in the order of positive electrode layer, inorganic solid electrolyte layer and negative electrode layer. After arrangement, they are packaged with aluminum-plastic film and isostatically pressed at a pressure of 100~1000MPa to obtain a soft-pack solid-state battery cell.

Citation Information

Patent Citations

  • Method for preparing nano silver carbon and application of nano silver carbon in lithium ion battery

    CN104577062A

  • Two-coat lithium ion battery negative electrode material, preparation method thereof and lithium ion battery

    CN107093710A

  • Bipolar laminated all-solid-state lithium-ion rechargeable battery and method for manufacturing same

    CN107180995A

  • High-air-stability inorganic sulfide solid electrolyte and preparation method and application thereof

    CN110085908A

  • Electrode structure, bipolar all-solid-state secondary battery including same, and method for manufacturing same

    CN114447263A