A doped perovskite-type adsorbent and preparation method thereof

By doping perovskite adsorbents, the micropore structure is improved and high-temperature sintering molding is used to solve the problem of reduced adsorption capacity and dissolution caused by granulation of lithium selective adsorbents, and efficient lithium adsorption effect is achieved.

CN118287035BActive Publication Date: 2024-11-22HUANENG CLEAN ENERGY RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410400654.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-03
Publication Date
2024-11-22
Estimated Expiration
2044-04-03

AI Technical Summary

Technical Problem

During the use of the existing lithium-selective adsorbent, the adsorption capacity decreases due to granulation, and there is a problem of dissolution loss, resulting in a significant decrease in the lithium adsorption capacity with the increase of the number of cycles.

Method used

Doped perovskite adsorbent, with the chemical formula H2-3xLaxMyTi1-yO3, improve the micropore structure by doping different elements, combined with high-temperature sintering molding, avoiding the capacity loss caused by granulation molding of traditional adsorbents and improving lithium Adsorption capacity and selectivity.

Benefits of technology

The lithium adsorbent has stable properties, low acid leach loss, and high lithium adsorption capacity and selectivity, avoiding the capacity loss of traditional adsorbents during recycling, and improving the adsorption efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118287035B_ABST
    Figure CN118287035B_ABST
Patent Text Reader

Abstract

The present invention relates to an adsorbent material for separating and extracting lithium from a salt lake, and in particular to a doped perovskite-type adsorbent and a preparation method thereof. The chemical formula of the doped perovskite-type adsorbent is H 2‑ 3x La x M y Ti 1‑y O3; wherein M is one or a mixture of Al, Ce, Sn, Nb, Zr, Mo, Ta, W, Pr and Hf, the value of x is greater than 0 and less than 2 / 3, and the value of y is greater than 0 and less than 0.5. The doped perovskite-type adsorbent of the present invention has stable properties and low acid leaching loss. At the same time, element doping increases the adsorption rate, and the molding is performed by high-temperature sintering, which avoids the capacity loss of traditional adsorbents caused by granulation molding, and has higher lithium adsorption capacity and lithium selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an adsorbent material for separating and extracting lithium from a salt lake, and in particular to a doped perovskite-type adsorbent and a preparation method thereof. Background Art

[0002] Lithium is known as the "white oil" of the future electrification era and is one of my country's 24 national strategic mineral resources. With the rapid development of the new energy industry, the global demand for lithium resources has grown rapidly, and the development and utilization of lithium resources has received more and more attention. At present, the monomer resource scale of lithium extraction from salt lakes is large, the operating cost is low, and the potential for technological advancement is large, making it an ideal source of lithium resources. Among various salt lake lithium extraction processes, the adsorption method can achieve low-grade and low-cost lithium extraction, and is the main technical route currently used.

[0003] The adsorption method uses a lithium selective adsorbent to adsorb lithium ions from brine, and then separates lithium ions from other competing cations through elution with a desorbent. The selective adsorbent is the core component, mainly including aluminum, manganese and titanium adsorbents. Although the existing adsorbent powder has a high adsorption capacity, the powder needs to be granulated in order to facilitate subsequent operations during actual use, resulting in a significant reduction in adsorption capacity. There are also problems such as dissolution loss, which causes the adsorption capacity to drop significantly with the increase in the number of cycles. Therefore, it is necessary to develop a moldable adsorbent with high adsorption performance. Summary of the invention

[0004] In order to overcome the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a doped perovskite-type adsorbent and a preparation method thereof. The doped perovskite-type adsorbent of the present invention has stable properties, low acid leaching loss, high lithium adsorption capacity and lithium selectivity, and high adsorption efficiency.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a doped perovskite-type adsorbent, wherein the chemical formula of the doped perovskite-type adsorbent is H 2-3x La x M y Ti 1-y O3; wherein M is one or a mixture of Al, Ce, Sn, Nb, Zr, Mo, Ta, W, Pr and Hf, the value of x is greater than 0 and less than 2 / 3, and the value of y is greater than 0 and less than 0.5.

[0007] Preferably, the raw materials for preparing the doped perovskite-type adsorbent include a lithium source, a lanthanum source, a titanium source, a doping metal source and an acid solution.

[0008] Preferably, the lithium source, lanthanum source, titanium source and doping metal source are any type of salt soluble in acid solution.

[0009] Preferably, the acid solution is an aqueous solution of an inorganic acid.

[0010] Preferably, the acid solution is an aqueous solution of an organic acid.

[0011] In a second aspect, the present invention provides a method for preparing a doped perovskite-type adsorbent, characterized in that it comprises the following steps:

[0012] Li 2-3x La x M y Ti 1-y The O3 molding material is subjected to acid elution to remove lithium to obtain the doped perovskite-type adsorbent.

[0013] Preferably, the Li 2-3x La x M y Ti 1-y The method for preparing the molding material of O3 comprises the following steps:

[0014] S1: dissolving lithium source, lanthanum source, titanium source and doping metal source in an acid solution, heating and drying to obtain a solid, and sintering to obtain Li 2-3x La x M y Ti 1-y O3 powder;

[0015] S2: Press the powder into a shape and sinter to obtain Li 2-3x La x M y Ti 1-y O3 molding material.

[0016] Preferably, the heating condition in S1 is: heating at 60-80°C for 10 min-6 h; and the drying condition is: heating at 80-150°C until the solution is completely dry.

[0017] Preferably, the sintering conditions in S1 are: sintering at 450-800°C for 2-8h, and then sintering at 1000-1250°C for 2-30h.

[0018] Preferably, the sintering conditions in S2 are: sintering at 900-1400° C. for 2-20 hours.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The chemical formula of the doped perovskite-type adsorbent of the present invention is H 2-3x La x M y Ti 1-yO3, wherein M is one or a mixture of Al, Ce, Sn, Nb, Zr, Mo, Ta, W, Pr and Hf. By doping different elements, the microporous structure of the adsorbent is improved and the adsorption rate is increased; the perovskite structure makes the adsorbent of the present invention stable in nature and low in acid leaching loss.

[0021] The present invention is formed by high-temperature sintering, thereby avoiding the capacity loss of traditional adsorbents caused by granulation molding, and has higher lithium adsorption capacity and lithium selectivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Schematic diagram of lithium adsorption capacity of the hydrogen-type adsorbent of the present invention;

[0023] Figure 2 This is a schematic diagram of the change in lithium adsorption capacity of the hydrogen-type adsorbent of the present invention after five cycles;

[0024] Figure 3 Schematic diagram of the magnesium-lithium ratio in the desorption solution of the present invention. DETAILED DESCRIPTION

[0025] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0026] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.

[0027] It should also be understood that the terms used in the present specification are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the present specification and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.

[0028] It should be further understood that the term "and / or" used in the present description and the appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.

[0029] Various structural schematic diagrams of the embodiments disclosed in the present invention are shown in the accompanying drawings. These figures are not drawn to scale, and some details are magnified and some details may be omitted for the purpose of clear expression. The shapes of various regions and layers shown in the figures and the relative sizes and positional relationships therebetween are only exemplary, and may deviate in practice due to manufacturing tolerances or technical limitations, and those skilled in the art may additionally design regions / layers with different shapes, sizes, and relative positions according to actual needs.

[0030] The first object of the present invention is to provide a doped perovskite-type adsorbent having a chemical formula of H 2-3x La x M y Ti 1- y O3; wherein M is one or a mixture of Al, Ce, Sn, Nb, Zr, Mo, Ta, W, Pr and Hf, the value of x is greater than 0 and less than 2 / 3, and the value of y is greater than 0 and less than 0.5. By doping a combination of different elements, the lattice parameters can be optimized and the structural distortion can be reduced on the basis of maintaining the perovskite structure, thereby improving the stability of the adsorbent.

[0031] The preparation raw materials of the invention include a lithium source, a lanthanum source, a titanium source, a doping metal source and an acid solution.

[0032] The perovskite structure type compound mentioned in the present invention mainly belongs to orthorhombic, cubic, rhombohedral, tetragonal, monoclinic and triclinic crystal systems. The A-site ion is usually a rare earth or alkaline earth metal element with a larger ionic radius. The present invention can be Li and La. The A-site ion is coordinated with 12 oxygens to form the closest cubic stacking, which mainly plays a role in stabilizing the perovskite structure; the B-site is generally an element with a smaller ionic radius (generally a transition metal element, such as Mn, Nb, Mo, Zr, Ta, W and Hf, etc.), and the present invention can also be a post-transition metal element, such as Al and Sn, or a lanthanide element, such as Ce and Pr; it can also be a mixture of multiple elements mentioned above, that is, a mixture of any of Al, Ce, Sn, Nb, Zr, Mo, Ta, W, Pr and Hf. The B-site ion is coordinated with 6 oxygens and occupies the octahedral center in the cubic close packing. Due to the variability of its valence state, it usually becomes the main component that determines many properties of the perovskite structure type material. Compared with simple oxides, the perovskite structure allows some elements to exist in abnormal valence states, or active metals to exist in mixed valence states, making the solid exhibit certain special properties.

[0033] The second object of the present invention is to provide a method for preparing a doped perovskite-type adsorbent, comprising the following steps:

[0034] Li 2-3x La xM y Ti 1-y The O3 molding material is subjected to acid elution to remove lithium to obtain the doped perovskite-type adsorbent.

[0035] Specifically: Li 2-3x La x M y Ti 1-y The O3 molding material is immersed in an acid solution and stirred to remove lithium to obtain H 2- 3x La x M y Ti 1-y O3 hydrogen type adsorbent.

[0036] Li 2-3x La x M y Ti 1-y The method for preparing the molding material of O3 comprises the following steps:

[0037] The lithium source, lanthanum source, titanium source and doping metal source are dissolved in an acid solution, heated and dried to obtain a solid, and sintered to obtain Li 2-3x La x M y Ti 1-y O3 powder; the powder is pressed into a shape to obtain Li 2-3x La x M y Ti 1-y O3 molding material.

[0038] Specifically, the lithium source, lanthanum source, titanium source and doping metal source are dissolved in an acid solution, heated at 60-80°C for 10min-6h, and then continued to heat at 80-150°C until the solution is completely dry; the obtained solid is sintered at 450-800°C for 2-8h, and then heated to 1000-1250°C at a rate of 5°C / min and sintered for 2-30h to obtain a white Li 2-3x La x M y Ti 1-y O3 powder; the obtained white powder is ball-milled for 4-24 hours, placed in a mold and pressed into a cylindrical shape, and then sintered at 900-1400℃ for 2-20 hours to obtain Li 2-3x La x M y Ti 1-y O3 molding material.

[0039] Among them, Li 2-3x La x M y Ti 1-yO3 can be prepared by solution-gel method, hydrothermal synthesis method and high-energy ball milling method. The lithium source, lanthanum source, titanium source and doping metal source can be any type of salt soluble in acid solution, and the acid can be any inorganic acid or organic acid.

[0040] The "number of parts" mentioned in the embodiments of the present invention refers to the molar ratio of each substance, which means to highlight the molar ratio relationship between the added substances, and does not limit the molar amount of the added substances. The molar amount can be more or less as long as the molar ratio is met.

[0041] Example 1

[0042] First, Li was prepared by the sol-gel method 0.29 La 0.57 Al 0.005 Ti 0.995 33 parts of LiNO3, 57 parts of La(NO3)3 and 0.5 parts of Al(NO3)3 were dissolved in 1L of 25% citric acid aqueous solution, 99.5 parts of tert-butyl titanium (IV) were added under vigorous stirring, and heated at 80°C for 10 minutes to obtain a uniform solution. The solution was heated to 150°C until it was completely dry, and the obtained solid was sintered at 600°C for 4 hours, then heated to 1100°C at a rate of 5°C / min and sintered for 20 hours to obtain white Li 0.29 La 0.57 Al 0.005 Ti 0.995 O3 powder.

[0043] The obtained white powder was ball-milled at 500 rpm for 12 hours, put into a tungsten carbide particle mold and pressed into a cylindrical shape with a diameter of 50 mm and a thickness of 70 mm, and then sintered at 1050° C. for 8 hours to obtain a molded material.

[0044] The obtained Li 0.29 La 0.57 Al 0.005 Ti 0.995 The O3 molding material was immersed in a 1 mol / L HCl solution and stirred for 30 min to obtain H 0.29 La 0.57 Al 0.005 Ti 0.995 O3 hydrogen type adsorbent.

[0045] Example 2

[0046] First, Li was prepared by the sol-gel method 0.29 La 0.57 Al 0.001 Ti 0.999O3. 29 parts of LiNO3, 57 parts of La(NO3)3 and 0.1 parts of Al(NO3)3 were dissolved in 1L of 25% citric acid aqueous solution, 99.9 parts of tert-butyl titanium (IV) were added under vigorous stirring, and heated at 80°C for 10 minutes to obtain a uniform solution. The solution was heated to 150°C until it was completely dry, and the obtained solid was sintered at 600°C for 4 hours, then heated to 1100°C at a rate of 5°C / min and sintered for 20 hours to obtain white Li 0.29 La 0.57 Al 0.001 Ti 0.999 O3 powder.

[0047] The obtained white powder was ball-milled at 500 rpm for 12 hours, put into a tungsten carbide particle mold and pressed into a cylindrical shape with a diameter of 50 mm and a thickness of 70 mm, and then sintered at 1050° C. for 8 hours to obtain a molded material.

[0048] The obtained Li 0.29 La 0.57 Al 0.001 Ti 0.999 The O3 molding material was immersed in a 1 mol / L HCl solution and stirred for 30 min to obtain H 0.29 La 0.57 Al 0.001 Ti 0.999 O3 hydrogen type adsorbent.

[0049] Example 3

[0050] First, Li was prepared by the sol-gel method 1.97 La 0.01 Ce 0.015 Ti 0.985 O3. 200 parts of LiNO3, 1 part of La(NO3)3 and 1.5 parts of CeCO3 were dissolved in 1L of 25% acetic acid aqueous solution, 98.5 parts of tert-butyl titanium (IV) were added under vigorous stirring, and heated at 60°C for 6 hours to obtain a uniform solution. The solution was heated to 80°C until it was completely dry, and the obtained solid was sintered at 450°C for 8 hours, then heated to 1000°C at a rate of 5°C / min and sintered for 30 hours to obtain white Li 1.97 La 0.01 Ce 0.015 Ti 0.985 O3 powder.

[0051] The obtained white powder was ball-milled at 100 rpm for 4 hours, put into a tungsten carbide particle mold and pressed into a cylindrical shape with a diameter of 50 mm and a thickness of 70 mm, and then sintered at 900° C. for 20 hours to obtain a molded material.

[0052] The obtained Li1.97 La 0.01 Ce 0.015 Ti 0.985 The O3 molding material was immersed in a 1 mol / L HCl solution and stirred for 30 min to obtain H 1.97 La 0.01 Ce 0.015 Ti 0.985 O3 hydrogen type adsorbent.

[0053] Example 4

[0054] First, Li was prepared by the sol-gel method 1.7 La 0.1 Zr 0.05 Ti 0.95 O3. 180 parts of LiNO3, 10 parts of La(NO3)3 and 5 parts of ZrCl4 were dissolved in 3L of 20% citric acid aqueous solution, 95 parts of tert-butyl titanium (IV) were added under vigorous stirring, and heated at 70°C for 3h to obtain a uniform solution. The solution was heated to 100°C until it was completely dry, and the obtained solid was sintered at 800°C for 2h, then heated to 1250°C at a rate of 5°C / min and sintered for 2h to obtain white Li 1.7 La 0.1 Zr 0.05 Ti 0.95 O3 powder.

[0055] The obtained white powder was ball-milled at 400 rpm for 24 hours, put into a tungsten carbide particle mold and pressed into a cylindrical shape with a diameter of 50 mm and a thickness of 70 mm, and then sintered at 1400° C. for 2 hours to obtain a molded material.

[0056] The obtained Li 1.7 La 0.1 Zr 0.05 Ti 0.95 The O3 molding material was immersed in a 1 mol / L HCl solution and stirred for 30 min to obtain H 1.7 La 0.1 Zr 0.05 Ti 0.95 O3 hydrogen type adsorbent.

[0057] Example 5

[0058] First, Li was prepared by the sol-gel method 1.4 La 0.2 Al 0.05 Ce 0.05 Ti 0.9O3. 150 parts of LiNO3, 20 parts of La(NO3)3, 5 parts of Al(NO3)3 and 5 parts of CeCO3 were dissolved in 1L of 25% citric acid aqueous solution, 90 parts of tert-butyl titanium (IV) were added under vigorous stirring, and heated at 75°C for 1h to obtain a uniform solution. The solution was heated to 120°C until it was completely dry, and the obtained solid was sintered at 500°C for 5 hours, then heated to 1200°C at a rate of 5°C / min and sintered for 25 hours to obtain white Li 1.4 La 0.2 Al 0.05 Ce 0.05 Ti 0.9 O3 powder.

[0059] The obtained white powder was ball-milled at 500 rpm for 20 hours, put into a tungsten carbide particle mold and pressed into a cylindrical shape with a diameter of 50 mm and a thickness of 70 mm, and then sintered at 1000° C. for 15 hours to obtain a molded material.

[0060] The obtained Li 1.4 La 0.2 Al 0.05 Ce 0.05 Ti 0.9 The O3 molding material was immersed in a 1 mol / L HCl solution and stirred for 30 min to obtain H 1.4 La 0.2 Al 0.05 Ce 0.05 Ti 0.9 O3 hydrogen type adsorbent.

[0061] Example 6

[0062] First, Li was prepared by the sol-gel method 1.1 La 0.3 Al 0.15 Ce 0.15 Ti 0.7 O3. 115 parts of LiNO3, 30 parts of La(NO3)3, 15 parts of Al(NO3)3 and 15 parts of ZrCl4 were dissolved in 1L of 25% citric acid aqueous solution, 70 parts of tert-butyl titanium (IV) were added under vigorous stirring, and heated at 65°C for 0.5h to obtain a uniform solution. The solution was heated to 80°C until it was completely dry, and the obtained solid was sintered at 700°C for 3 hours, then heated to 1100°C at a rate of 5°C / min and sintered for 20 hours to obtain white Li 1.1 La 0.3 Al 0.15 Ce 0.15 Ti 0.7 O3 powder.

[0063] The obtained white powder was ball-milled at 500 rpm for 8 hours, put into a tungsten carbide particle mold and pressed into a cylindrical shape with a diameter of 50 mm and a thickness of 70 mm, and then sintered at 1300° C. for 6 hours to obtain a molded material.

[0064] The obtained Li 1.1 La 0.3 Al 0.15 Ce 0.15 Ti 0.7 The O3 molding material was immersed in a 1 mol / L HCl solution and stirred for 30 min to obtain H 1.1 La 0.3 Al 0.15 Ce 0.15 Ti 0.7 O3 hydrogen type adsorbent.

[0065] Example 7

[0066] First, Li was prepared by the sol-gel method 0.8 La 0.4 Zr 0.25 Ce 0.25 Ti 0.5 O3. 90 parts of LiNO3, 40 parts of La(NO3)3, 25 parts of ZrCl4 and 25 parts of CeCO3 were dissolved in 1L of 25% citric acid aqueous solution, 50 parts of tert-butyl titanium (IV) were added under vigorous stirring, and heated at 65°C for 1h to obtain a uniform solution. The solution was heated to 100°C until it was completely dry, and the obtained solid was sintered at 500°C for 7 hours, then heated to 1200°C at a rate of 5°C / min and sintered for 10 hours to obtain white Li 0.8 La 0.4 Zr 0.25 Ce 0.25 Ti 0.5 O3 powder.

[0067] The obtained white powder was ball-milled at 400 rpm for 20 hours, put into a tungsten carbide particle mold and pressed into a cylindrical shape with a diameter of 50 mm and a thickness of 70 mm, and then sintered at 1150° C. for 10 hours to obtain a molded material.

[0068] The obtained Li 0.8 La 0.4 Zr 0.25 Ce 0.25 Ti 0.5 The O3 molding material was immersed in a 1 mol / L HCl solution and stirred for 30 min to obtain H 0.8 La 0.4 Zr 0.25 Ce 0.25 Ti 0.5O3 hydrogen type adsorbent.

[0069] Example 8

[0070] First, Li was prepared by the sol-gel method 0.5 La 0.5 Al 0.1 Zr 0.1 Ce 0.1 Ti 0.7 O3. Mix 53 parts of LiNO3, 50 parts of La(NO3)3, and 10 parts of Al(NO3) 3、 10 parts of ZrCl4 and 10 parts of CeCO3 were dissolved in 1L of 25% citric acid aqueous solution, and 70 parts of tert-butyl titanium (IV) were added under vigorous stirring, and heated at 80°C for 10 minutes to obtain a uniform solution. The solution was heated to 140°C until it was completely dry, and the obtained solid was sintered at 600°C for 4 hours, and then heated to 1100°C at a rate of 5°C / min and sintered for 20 hours to obtain white Li 0.5 La 0.5 Al 0.1 Zr 0.1 Ce 0.1 Ti 0.7 O3 powder.

[0071] The obtained white powder was ball-milled at 500 rpm for 22 hours, put into a tungsten carbide particle mold and pressed into a cylindrical shape with a diameter of 50 mm and a thickness of 70 mm, and then sintered at 1275° C. for 12 hours to obtain a molded material.

[0072] The obtained Li 0.5 La 0.5 Al 0.1 Zr 0.1 Ce 0.1 Ti 0.7 The O3 molding material was immersed in a 1 mol / L HCl solution and stirred for 30 min to obtain H 0.5 La 0.5 Al 0.1 Zr 0.1 Ce 0.1 Ti 0.7 O3 hydrogen type adsorbent.

[0073] Example 9

[0074] First, Li was prepared by the sol-gel method 0.2 La 0.6 Al 0.1 Ti 0.9O3. 22 parts of LiNO3, 60 parts of La(NO3)3 and 10 parts of Al(NO3)3 were dissolved in 1L of 25% citric acid aqueous solution, 90 parts of tert-butyl titanium (IV) were added under vigorous stirring, and heated at 75°C for 1h to obtain a uniform solution. The solution was heated to 150°C until it was completely dry, and the obtained solid was sintered at 600°C for 4 hours, then heated to 1100°C at a rate of 5°C / min and sintered for 20 hours to obtain white Li 0.2 La 0.6 Al 0.1 Ti 0.9 O3 powder.

[0075] The obtained white powder was ball-milled at 500 rpm for 12 hours, put into a tungsten carbide particle mold and pressed into a cylindrical shape with a diameter of 50 mm and a thickness of 70 mm, and then heated at 1300° C. for 6 hours to obtain a molded material.

[0076] The obtained Li 0.2 La 0.6 Al 0.1 Ti 0.9 The O3 molding material was immersed in a 1 mol / L HCl solution and stirred for 30 min to obtain H 0.2 La 0.6 Al 0.1 Ti 0.9 O3 hydrogen type adsorbent.

[0077] Example 10

[0078] First, Li was prepared by the sol-gel method 0.05 La 0.65 Al 0.2 Ti 0.8 O3. 8 parts of LiNO3, 65 parts of La(NO3)3 and 20 parts of Al(NO3)3 were dissolved in 1L of 25% citric acid aqueous solution, 80 parts of tert-butyl titanium (IV) were added under vigorous stirring, and heated at 60°C for 6h to obtain a uniform solution. The solution was heated to 80°C until it was completely dry, and the obtained solid was sintered at 800°C for 3 hours, then heated to 1150°C at a rate of 5°C / min and sintered for 15 hours to obtain white Li 0.05 La 0.65 Al 0.2 Ti 0.8 O3 powder.

[0079] The obtained white powder was ball-milled at 500 rpm for 16 hours, put into a tungsten carbide particle mold and pressed into a cylindrical shape with a diameter of 50 mm and a thickness of 70 mm, and then sintered at 1200° C. for 15 hours to obtain a molded material.

[0080] The obtained Li0.05 La 0.65 Al 0.2 Ti 0.8 The O3 molding material was immersed in a 1 mol / L HCl solution and stirred for 30 min to obtain H 0.05 La 0.65 Al 0.2 Ti 0.8 O3 hydrogen type adsorbent.

[0081] Take 1000 mL of brine with the composition shown in Table 1, adjust the pH to 8.0 with 0.1 mol / L NaOH solution, add 50 g of hydrogen-type adsorbent prepared in Examples 1-3, soak for 60 min under stirring, filter, and obtain adsorption mother solution L1. Determine its Li + Mg 2 + The filter cake S1 is loaded with Li + adsorbent; add 100 mL of 1.0 mol / L hydrochloric acid to S1, soak for 30 min under stirring, filter, and obtain desorption solution L2. Determine its Li + Mg 2+ The filter cake S2 ​​obtained is a hydrogen-type adsorbent, which can be recycled.

[0082] Table 1 Component content of brine

[0083] Components <![CDATA[Na + ]]> <![CDATA[K + ]]> <![CDATA[Mg 2+ ]]> <![CDATA[Ca 2+ ]]> <![CDATA[Li + ]]> <![CDATA[B 3+ ]]> <![CDATA[SO4 2- ]]> <![CDATA[Cl - ]]> Mg / Li ratio Content (g / L) 79.56 9.84 17.4 0.72 0.18 0.19 6.48 192.84 96.67

[0084] like Figure 1 , 2 As shown in 3, Figure 1 is the lithium adsorption capacity of the adsorption mother solution L1; Figure 2 is the lithium adsorption capacity after five cycles of adsorption of mother solution L1; Figure 3 is the magnesium-lithium ratio in the desorption solution L2.

[0085] It can be seen that the hydrogen-type adsorbent material obtained by the present invention has a higher lithium adsorption capacity and cyclic stability, avoiding the capacity loss of traditional adsorbents during the granulation process and the dissolution problem during the acid treatment process; at the same time, the magnesium and lithium in the analysis solution are relatively low, which meets the standards for separating and extracting lithium from salt lake brine.

[0086] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A doped perovskite-type adsorbent, characterized in that: Li 2-3x La x M y Ti 1-y The method for preparing the molding material of O3 comprises the following steps: S1: dissolving lithium source, lanthanum source, titanium source and doping metal source in an acid solution, heating and drying to obtain a solid, and sintering to obtain Li 2-3x La x M y Ti 1-y O3 powder; S2: Press the powder into a shape and sinter to obtain Li 2-3x La x M y Ti 1-y O3 molding materials; Li 2-3x La x M y Ti 1-y The O3 molding material is subjected to acid elution to remove lithium to obtain the doped perovskite-type adsorbent; The chemical formula of the doped perovskite-type adsorbent is H 2-3x La x M y Ti 1-y O3; wherein M is one or a mixture of Al, Ce, Sn, Nb, Zr, Mo, Ta, W, Pr and Hf, the value of x is greater than 0 and less than 2 / 3, and the value of y is greater than 0 and less than 0.5; The lithium source, lanthanum source, titanium source and doping metal source are any type of salts soluble in an acid solution.

2. A doped perovskite-type adsorbent according to claim 1, characterized in that: The acid solution is an aqueous solution of an inorganic acid.

3. The doped perovskite-type adsorbent according to claim 1, characterized in that: The acid solution is an aqueous solution of an organic acid.

4. A method for preparing a doped perovskite-type adsorbent according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1: dissolving lithium source, lanthanum source, titanium source and doping metal source in an acid solution, heating and drying to obtain a solid, and sintering to obtain Li 2-3x La x M y Ti 1-y O3 powder; S2: Press the powder into a shape and sinter to obtain Li 2-3x La x M y Ti 1-y O3 molding materials; Li 2-3x La x M y Ti 1-y The O3 molding material is subjected to acid elution to remove lithium to obtain the doped perovskite-type adsorbent.

5. The method for preparing a doped perovskite-type adsorbent according to claim 4, characterized in that: The heating conditions of S1 are: heating at 60-80°C for 10 min-6 h; the drying conditions are: heating at 80-150°C until the solution is completely dry.

6. The method for preparing a doped perovskite-type adsorbent according to claim 4, characterized in that: The sintering conditions in S1 are: sintering at 450-800°C for 2-8h, and then sintering at 1000-1250°C for 2-30h.

7. The method for preparing a doped perovskite-type adsorbent according to claim 4, characterized in that: The sintering conditions described in S2 are: sintering at 900-1400° C. for 2-20 hours.