A-TIG welding activator based on 2205 duplex stainless steel

By using a specific ratio of A-TIG welding activator, the problems of uneven weld appearance, unstable arc and improper welding parameters are solved, and the yield strength, tensile strength and hardness of the weld are significantly improved, and the weld is achieved Improved quality and performance to meet design requirements.

CN118287890BActive Publication Date: 2024-10-15ZHANGJIAJIE INST OF AERONAUTICAL ENG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410577374.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-10
Publication Date
2024-10-15
Estimated Expiration
2044-05-10

AI Technical Summary

Technical Problem

In the existing A-TIG welding technology, the appearance of the weld is uneven, the arc is unstable, the welding parameters are improper, the weld does not penetrate, the tensile strength and impact toughness are low, and the heat-affected zone is too wide, which affects the microstructure and performance of the metal.

Method used

Use 2205 duplex stainless steel A-TIG welding activator composed of SiO2 powder, Cr2O3 powder, Al2O3 powder, TiO2 powder, MnO2 powder, Y2O3 powder, NaCl powder, B2O3 powder, MgO powder, CuO powder, through uniform coating and Evaporate absolute ethanol before welding and then weld to form an excellent microstructure of the weld and improve the yield strength, tensile strength and hardness of the weld.

Benefits of technology

The weld surface is smooth, the tensile strength, impact toughness and fatigue strength are better than the base metal, meeting the design requirements. The mechanical properties of the heat-affected zone are close to the base metal, there are no structural weaknesses, and the weld quality is high and defect-free.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118287890B_ABST
    Figure CN118287890B_ABST
Patent Text Reader

Abstract

The invention discloses an A-TIG welding activator based on 2205 duplex stainless steel, belonging to the technical field of metal welding; the A-TIG welding activator is composed of the following mass percentages: SiO 2 Powder 20~40%, Cr 2 O 3 Powder 20-30%, Al 2 O 3 Powder 10-30%, TiO 2 Powder 5-10%, MnO 2 Powder 15-30%, Y 2 O 3 Powder 5-10%, NaCl powder 5-10%; B 2 O 3 Powder 3-10%, MgO powder 2-10%, CuO powder 3-10%; after using this activator, the precipitation of austenite from ferrite in the weld microstructure is more mature, the organizational performance is excellent, and the yield strength and tensile strength of the weld are significantly improved; the weld hardness is significantly improved, which is of great significance for A-TIG welding based on 2205 duplex stainless steel and has excellent application and promotion prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal welding, and in particular to an A-TIG welding activator based on 2205 duplex stainless steel. Background Art

[0002] As a new welding technology, A-TIG welding is widely used at home and abroad. However, foreign countries have strict confidentiality requirements on the proportion of welding active agent formula. Therefore, it is of great significance to explore and study the more mature welding process parameters of A-TIG.

[0003] In the prior art, SiO2 powder, Cr2O3 powder, Al2O3 powder, TiO2 powder, MnO2 powder, Y2O3 powder, and B2O3 powder are disclosed as welding activators. However, this solution has the following problems during the welding process:

[0004] 1. The surface of the weld is uneven. The arc is unstable during the welding process, and there is spatter, which affects the appearance and surface strength of the structure, and requires a long time of grinding in the later stage.

[0005] 2. Improper welding parameters can easily lead to the weld failing to penetrate the entire thickness of the workpiece, resulting in a decrease in the bearing capacity of the welded structure.

[0006] 3. The tensile strength and impact toughness of the welding area are easily lower than the base material or design requirements, and the tensile strength and impact toughness of the weld are not high.

[0007] 4. Excessive heat input causes the heat affected zone to be too wide, thus affecting the microstructure and properties of the metal.

[0008] Therefore, there is an urgent need for an A-TIG welding activator formula with better performance based on 2205 duplex stainless steel, so that the performance of the weld can be significantly improved. Summary of the invention

[0009] The invention aims to overcome the disadvantages of the prior art and provides an A-TIG welding activator based on 2205 duplex stainless steel, belonging to the technical field of metal welding; the A-TIG welding activator is composed of the following mass percentages: 20-40% of SiO2 powder, 20-30% of Cr2O3 powder, 10-30% of Al2O3 powder, 5-10% of TiO2 powder, 15-30% of MnO2 powder, 5-10% of Y2O3 powder, 5-10% of NaCl powder; 3-10% of B2O3 powder, 2-10% of MgO powder, and 3-10% of CuO powder; after using the activator, austenite in the microstructure of the weld is more maturely precipitated from ferrite, the microstructure performance is excellent, the yield strength and tensile strength of the weld are significantly improved, and the hardness of the weld is significantly improved, which is of great significance for A-TIG welding based on 2205 duplex stainless steel and has excellent application and promotion prospects.

[0010] In order to achieve the above technical effects, the following technical solutions are adopted:

[0011] The invention discloses an A-TIG welding activator based on 2205 duplex stainless steel, which is composed of the following mass percentages: 20-40% of SiO2 powder, 20-30% of Cr2O3 powder, 10-30% of Al2O3 powder, 5-10% of TiO2 powder, 15-30% of MnO2 powder, 5-10% of Y2O3 powder, 5-10% of NaCl powder; 3-10% of B2O3 powder, 2-10% of MgO powder, and 3-10% of CuO powder.

[0012] Furthermore, the active agent is composed of the following mass percentages: SiO2 powder 20%, Cr2O3 powder 20%, Al2O3 powder 10%, TiO2 powder 5%, MnO2 powder 20%, Y2O3 powder 5%, NaCl powder 5%; B2O3 powder 3%, MgO powder 2%, CuO powder 10%.

[0013] Furthermore, the active agent is composed of the following mass percentages: 30% SiO2 powder, 20% Cr2O3 powder, 10% Al2O3 powder, 5% TiO2 powder, 15% MnO2 powder, 5% Y2O3 powder, 5% NaCl powder; 5% B2O3 powder, 2% MgO powder, and 3% CuO powder.

[0014] Furthermore, the active agent is composed of the following mass percentages: SiO2 powder 25%, Cr2O3 powder 20%, Al2O3 powder 10%, TiO2 powder 5%, MnO2 powder 17.5%, Y2O3 powder 5%, NaCl powder 5%; B2O3 powder 4%, MgO powder 2%, CuO powder 6.5%.

[0015] Furthermore, the method for using the activator is as follows: before welding begins, ensure that the welding surface of the 2205 duplex stainless steel is clean, free of grease or other contaminants, and use an angle grinder or sandpaper to remove the surface oxide film; then use a soft brush or special spraying equipment to evenly apply the prepared activator to the welding area, and control the coating thickness to just cover the metal base material, and do not apply too much to avoid waste or potential welding defects; finally, wait for the anhydrous ethanol in the activator to completely evaporate before welding.

[0016] Furthermore, the preparation method of the active agent is: using an electronic balance to mix the active agent powder with a mass ratio of 90% to 95% and the anhydrous ethanol with a mass ratio of 5% to 10%, stirring evenly, and preparing a paste or viscous liquid.

[0017] Application of the above activator in A-TIG welding of 2205 duplex stainless steel.

[0018] The beneficial effects of the present invention are:

[0019] (1) The weld surface is flat and smooth, without excessive protrusions and depressions, the weld toe is smooth and transitional, and there is not much spatter, meeting the aesthetic and functional requirements.

[0020] (2) The weld quality is high, without any welding defects such as cracks, holes, slag inclusions, and incomplete penetration.

[0021] (3) The tensile strength, impact toughness and fatigue strength of the weld are better than those of the parent material and meet the design requirements.

[0022] (4) The mechanical properties of the heat-affected zone are similar to those of the parent material, and there are no structural weaknesses. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. The drawings in the following description are merely embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.

[0024] Figure 1 The macroscopic morphology of the front and back sides of the weld of 2205 duplex stainless steel using activator 4 in the embodiment of the present invention;

[0025] Figure 2 The macroscopic morphology of the front and back sides of the weld of 2205 duplex stainless steel using activator 1 in the embodiment of the present invention;

[0026] Figure 3 The microstructure diagram of different penetration depths in the center of the weld using activator 4 in the embodiment of the present invention;

[0027] Figure 4 The microstructure diagram of different penetration depths in the center of the weld using activator 1 in the embodiment of the present invention;

[0028] Figure 5 This is a comparison chart of A-Tig weld hardness curves using different activators 4 in the embodiments of the present invention.

[0029] Figure 6 This is a schematic diagram of active agent coating welding in an embodiment of the present invention. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0031] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0032] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations and / or combinations thereof.

[0033] Embodiment 1:

[0034] The active agent ratio used in this embodiment is as follows:

[0035] Active agent 1: composed of the following mass percentages: SiO2 powder 20%, Cr2O3 powder 20%, Al2O3 powder 10%, TiO2 powder 5%, MnO2 powder 20%, Y2O3 powder 5%, NaCl powder 5%; B2O3 powder 3%, MgO powder 2%, CuO powder 10%.

[0036] Active agent 2: composed of the following mass percentages: SiO2 powder 30%, Cr2O3 powder 20%, Al2O3 powder 10%, TiO2 powder 5%, MnO2 powder 15%, Y2O3 powder 5%, NaCl powder 5%; B2O3 powder 5%, MgO powder 2%, CuO powder 3%.

[0037] Active agent 3: composed of the following mass percentages: SiO2 powder 25%, Cr2O3 powder 20%, Al2O3 powder 10%, TiO2 powder 5%, MnO2 powder 17.5%, Y2O3 powder 5%, NaCl powder 5%; B2O3 powder 4%, MgO powder 2%, CuO powder 6.5%.

[0038] Take activator 1, activator 2 and activator 3 for welding test: mix activator powder with a mass ratio of 90% to 95% and anhydrous ethanol with a mass ratio of 5% to 10% together, stir evenly in a beaker with a glass rod, and prepare a paste or viscous liquid. Ensure that the welding surface of 2205 duplex stainless steel is clean, free of grease or other pollutants, and use an angle grinder or sandpaper to remove the surface oxide film; then use a soft brush or special spraying equipment to evenly apply the prepared activator to the welding area, and control the coating thickness to just cover the metal base material. Do not apply too much to avoid waste or potential welding defects; finally, wait for the anhydrous ethanol in the activator to completely evaporate before welding. Figure 6 shown.

[0039] The material used in the test is 4-8 mm 2205 duplex stainless steel plate, the mechanical properties are shown in Table 1, the welding process parameters are shown in Table 2, and the specimen size is 150 mm × 60 mm × 4 mm to 150 mm × 60 mm × 8 mm.

[0040] Table 1 Mechanical properties of 2205 duplex stainless steel

[0041]

[0042] Table 2 Welding process parameters

[0043]

[0044] Comparative Example 1:

[0045] Active agent 4: composed of the following mass percentages: SiO2 powder 20%, Cr2O3 powder 20%, Al2O3 powder 10%, TiO2 powder 15%, MnO2 powder 20%, Y2O3 powder 10%; B2O3 powder 5%.

[0046] Active agent 5: composed of the following mass percentages: SiO2 powder 20%, Cr2O3 powder 20%, Al2O3 powder 10%, TiO2 powder 5%, MnO2 powder 20%, Y2O3 powder 10%; B2O3 powder 3%, MgO powder 2%, CuO powder 10%.

[0047] Active agent 6: composed of the following mass percentages: SiO2 powder 20%, Cr2O3 powder 20%, Al2O3 powder 10%, TiO2 powder 5%, MnO2 powder 20%, Y2O3 powder 5%, NaCl powder 5%; B2O3 powder 5%, CuO powder 10%.

[0048] Active agent 7: composed of the following mass percentages: SiO2 powder 20%, Cr2O3 powder 20%, Al2O3 powder 10%, TiO2 powder 5%, MnO2 powder 20%, Y2O3 powder 15%, NaCl powder 5%; B2O3 powder 3%, MgO powder 2%.

[0049] Welding tests were conducted using activators 4, 5, 6 and 7:

[0050] The material used in the test is 4-8 mm 2205 duplex stainless steel plate, the mechanical properties are shown in Table 1, the welding process parameters are shown in Table 2, and the specimen size is 150 mm × 60 mm × 4 mm to 150 mm × 60 mm × 8 mm.

[0051] Comparison of weld performance under different activator schemes:

[0052] 1. Comparison of weld appearance

[0053] Figure 1 shows the macroscopic morphology of the front and back sides of the weld of 2205 duplex stainless steel after welding with activator 4. When the weld reaches the coating area, the test plate is welded through, accompanied by black dot-shaped slag, and the weld bead on the back is well formed. Figure 2 shows the macroscopic morphology of the front and back sides of the weld of 2205 duplex stainless steel after welding with activator 1. It can be seen from the figure that the weld bead is obviously narrowed in the coating area, the surface is beautifully formed, the fish corrugation is uniform, and the front weld bead is slightly concave.

[0054] After analysis, it is found that the activator is coated on the surface of the base material. Under the influence of the welding heat field, part of the activator components will evaporate to form an ion field, which will affect the arc contraction; the other part will enter the welding molten pool and affect the fluidity of the molten pool. Therefore, the analysis shows that the chemical elements added in the weld are all from the chemical composition of the activator. O, Na, Mg, etc. are very strong surface active elements, which can make the weld molten pool produce a positive surface tension temperature gradient, and Fe, Cu, Cr, Si, etc. can cause the arc to contract. Under the combined effect of these two reasons, after welding with activator 1, the weld penetration is greatly increased.

[0055] 2. Microstructure comparison

[0056] 2.1 Metallographic analysis

[0057] like Figure 3As shown in the figure, after welding with activator 4, the weld microstructure is composed of dark gray ferrite and white austenite, and it can be seen that there are strip-shaped intragranular austenite and Widmanstätten austenite precipitation inside the dark gray ferrite. The grain size, size and shape of ferrite in the weld are different, and they are distributed in the form of strips, short rods and nearly equiaxed shapes. This is because 2205 duplex steel solidifies in the form of ferrite after melting, and most of the welds are ferrite structures. Austenite mainly precipitates from ferrite and exists in the form of short columns and trees.

[0058] like Figure 4 As shown, after welding with activator 1, the cooling rate of the weld slows down, the diffusion of elements and the structural transformation of the crystal are more mature, the austenite gradually changes from thin strips to coarser, and the ferrite structure also gradually grows, that is, it changes from slender columnar crystals to large equiaxed crystals. The equiaxed ferrite crystals can precipitate more austenite structure, and the precipitation of austenite from ferrite in the microstructure is more mature, and the organizational performance is more excellent.

[0059] 3. Comparison of mechanical properties

[0060] 3.1 Bending test

[0061] Table 3 Results of bending test after welding using activators 4-7

[0062]

[0063] Table 4 Results of bending tests after welding using activators 1-3

[0064]

[0065]

[0066] As shown in Table 3 and Table 4, in accordance with the requirements of GB / T2653-2008 standard, the weld joints were subjected to face bending and back bending tests. The diameter of the pressure head was 4 times the thickness of the specimen. After bending 180°, the activators 4-7 showed obvious face and back crack defects, while the activators 1-3 met the requirements of the specification and had high reliability.

[0067] 3.2 Tensile test

[0068] The tensile test of welded joints and the tensile test of weld metal are carried out in accordance with the standards of "Transverse Tensile Test of Metallic Materials Welds for Destructive Test" (GB / T 2651-2023) and "Longitudinal Tensile Test of Metallic Materials Welds for Destructive Test" (GB / T2652-2023) respectively.

[0069] Table 5 A-TIG welding tensile test results using activators 4-7

[0070]

[0071] Table 6 A-TIG welding tensile test results using activators 1-3

[0072]

[0073] As shown in Tables 5 and 6, the tensile test results of A-TIG welding using activators 1-3 are significantly better than those of A-TIG welding using activators 4-7.

[0074] 3.3 Hardness test

[0075] Figure 5 This is a comparison chart (Brinell hardness) of the A-Tig weld hardness curves using activator 4, activator 5, activator 6, activator 7 and activator 1. It can be seen that when activator 1 is used, the A-Tig weld hardness curve is significantly better than the A-Tig weld hardness curves using activators 4-7.

[0076] 4. Comparison of chemical properties

[0077] Si plays a role of deoxidation in carbon steel. During the welding process, it can effectively remove the harmful gases remaining in the weld, prevent the formation of pores and oxides, and can also refine the grains, thereby increasing the strength of the steel, while reducing its plasticity and toughness. Mn also has a good deoxidation effect. After solution treatment, it can increase the tensile strength and cold work hardening of the weld. Mn can also promote the growth of austenite grains in the weld. Coarse grain structure will reduce the plasticity and toughness of the material, and reduce the ability of the weld metal to resist external impact loads.

[0078] Through the test and analysis of the chemical composition of the welded joints, the chemical composition of the welds obtained by using the activator formulations 1-3 is compared with the chemical composition of the welds obtained by using the activator formulations 4-7, and the content of Cr, Ni, and Mo elements are increased, which can improve the corrosion resistance of duplex stainless steel, as shown in Table 7.

[0079] Table 7 Chemical composition of A-TIG welds using activators 1-3 (mass fraction / %)

[0080]

[0081] Table 8 Chemical composition of A-TIG weld using activating agent 4-7 (mass fraction / %)

[0082]

[0083] In summary, the present invention discloses an A-TIG welding activator based on 2205 duplex stainless steel, belonging to the technical field of metal welding; the A-TIG welding activator is composed of the following mass percentages: 20-40% SiO2 powder, 20-30% Cr2O3 powder, 10-30% Al2O3 powder, 5-10% TiO2 powder, 15-30% MnO2 powder, 5-10% Y2O3 powder, 5-10% NaCl powder; 3-10% B2O3 powder, 2-10% MgO powder, 3-10% CuO powder; after using the activator, austenite in the weld microstructure precipitates more maturely from ferrite, the organizational properties are excellent, and the yield strength and tensile strength of the weld are significantly improved; the weld hardness is significantly improved, which is of great significance for A-TIG welding based on 2205 duplex stainless steel and has excellent application and promotion prospects.

[0084] At this point, those skilled in the art recognize that, although the embodiments of the present invention have been shown and described in detail herein, many other variations or modifications that conform to the principles of the present invention can still be directly determined or derived based on the contents disclosed in the present invention without departing from the spirit and scope of the present invention. Therefore, the scope of the present invention should be understood and recognized as covering all such other variations or modifications.

Claims

1. A-TIG welding activator based on 2205 duplex stainless steel, It is characterized in that The active agent preparation method is: Using an electronic balance, 90% to 95% of the active agent powder and 5% to 10% of anhydrous ethanol are mixed together, stirred evenly, and a paste or viscous liquid is prepared; The active agent powder is composed of the following mass percentages: SiO 2 Powder 20-30%, Cr 2 O 3 Powder 20-30%, Al 2 O 3 Powder 10%, TiO 2 Powder 5-10%, MnO 2 Powder 15-20%, Y 2 O 3 Powder 5-10%, NaCl powder 5-10%; B 2 O 3 Powder 3-10%, MgO powder 2-10%, CuO powder 3-10%.

2. An A-TIG welding activator based on 2205 duplex stainless steel as claimed in claim 1, It is characterized in that The active agent powder is composed of the following mass percentages: SiO 2 Powder 20%, Cr 2 O 3 Powder 20%, Al 2 O 3 Powder 10%, TiO 2 Powder 5%, MnO 2 Powder 20%, Y 2 O 3 Powder 5%, NaCl powder 5%; B 2 O 3 Powder 3%, MgO powder 2%, CuO powder 10%.

3. An A-TIG welding activator based on 2205 duplex stainless steel as claimed in claim 1, It is characterized in that The active agent powder is composed of the following mass percentages: SiO 2 Powder 30%, Cr 2 O 3 Powder 20%, Al 2 O 3 Powder 10%, TiO 2 Powder 5%, MnO 2 Powder 15%, Y 2 O 3 Powder 5%, NaCl powder 5%; B 2 O 3 Powder 5%, MgO powder 2%, CuO powder 3%.

4. A-TIG welding activator based on 2205 duplex stainless steel as claimed in claim 1, It is characterized in that The active agent powder is composed of the following mass percentages: SiO 2 Powder 25%, Cr 2 O 3 Powder 20%, Al 2 O 3 Powder 10%, TiO 2 Powder 5%, MnO 2 Powder 17.5%, Y 2 O 3 Powder 5%, NaCl powder 5%; B 2 O 3 Powder 4%, MgO powder 2%, CuO powder 6.5%.

5. A-TIG welding activator based on 2205 duplex stainless steel as claimed in claim 1, It is characterized in that The method for using the activator is as follows: before welding, ensure that the welding surface of 2205 duplex stainless steel is clean, free of grease or other contaminants, and use an angle grinder or sandpaper to remove the surface oxide film; then use a soft brush or special spraying equipment to evenly apply the prepared activator to the welding area, and control the coating thickness to just cover the metal base material, and do not apply too much to avoid waste or potential welding defects; finally, wait for the anhydrous ethanol in the activator to completely volatilize before welding.