Two-dimensional layered material and preparation method thereof, positive electrode sheet and lithium ion battery
By using expandable two-dimensional layered materials as conductive agents in lithium-ion batteries, the problem of insufficient oxygen capture at high temperatures is solved, the safety and conductivity of the battery are improved, and the energy density is not affected at low temperatures, realizing the Adaptation of different cathode material systems.
Patent Information
- Application Number
- CN202410711576.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-04
AI Technical Summary
Existing lithium-ion batteries have insufficient active oxygen capture capabilities of cathode materials at high temperatures, leading to safety hazards, and traditional coating materials affect conductivity and battery performance.
Expandable two-dimensional layered materials are used as conductive agents. By embedding metal elements or inorganic compounds, the layer spacing and expansion characteristics are controlled to improve the ability to capture oxygen at high temperatures. At the same time, the small size does not affect the energy density at low temperatures.
At low addition amounts, it significantly improves the oxygen capture capacity, increases the surface area, ensures battery safety, and has good conductivity without affecting battery performance, and is suitable for different cathode material systems.
Smart Images

Figure CN118289802B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to two-dimensional layered materials and preparation methods thereof, positive electrodes and lithium-ion batteries. Background Art
[0002] In recent years, driven by pure electric vehicles and smartphones, the energy density of lithium-ion batteries has continued to increase. At present, the energy density of Beijing Weilan's mass-produced soft-pack batteries has reached 360Wh / kg. To achieve such a high energy density, the positive electrode material needs to use lithium cobalt oxide or ternary materials with a very high gram capacity. These materials have poor stability and will decompose and release oxygen at high temperatures. Oxygen reacts with ethylene carbonate (EC), the main component of the electrolyte, to release heat. At the same time, some oxygen diffuses to the negative electrode through the diaphragm and reacts with the lithium-embedded negative electrode, further releasing a large amount of heat, causing the battery to catch fire and explode.
[0003] In order to improve the safety of lithium cobalt oxide and ternary materials, it is necessary to capture the active oxygen released by their decomposition at high temperatures. Xinwanda Electric Vehicle Battery Co., Ltd. applied for the Chinese invention patent CN 110071278 A "A high-nickel ternary cathode material containing an active oxygen remover and its preparation method", using transition metal disulfide (MS2) to coat high-nickel materials and react with the active oxygen released by the cathode to improve circulation and high-temperature storage. However, MS2 is an inorganic material and it is difficult to coat evenly; and the volume of high-nickel materials changes greatly during the cycle, causing damage to the coating layer. At the same time, MS2 is a semiconductor, which affects the transmission of electrons in the cathode, increases the internal resistance of the battery, and reduces the rate performance. The Chinese utility model patent CN211088320U "Lithium-ion battery" applied by Hunan Xinminya New Energy Technology Co., Ltd. (Lingpai New Energy) uses an expandable graphite coating, which expands after the battery is heated to wrap the battery cell and isolate the air. However, the coating is coated on the inner wall of the battery shell. Its main function is to extinguish the fire when thermal runaway has occurred to avoid heat diffusion, and it cannot change the safety of the battery cell itself. At the same time, according to the literature (Energy Storage Materials, 2021, 39, 395-402), once the battery reaches the condition of thermal runaway, even the use of liquid nitrogen cannot stop the thermal runaway. Considering that the volume of the expanded graphite inside the battery cell is less than 10%, the final effect may be lower than expected.
[0004] In view of this, there is an urgent need to invent a method that can improve the intrinsic safety of batteries, which can capture active oxygen at high temperatures on the one hand, and on the other hand has a smaller volume at low temperatures and hardly affects the energy density of the battery. Summary of the invention
[0005] In view of this, the present invention provides a two-dimensional layered material and a preparation method thereof, a positive electrode sheet and a lithium-ion battery. The two-dimensional layered material expands at high temperatures, improving the ability to capture oxygen and ensuring battery safety; at the same time, the volume is small at low temperatures, which hardly affects the energy density of the battery.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] In a first aspect, the present invention provides a two-dimensional layered material, the molecular formula of which is A n MX2;
[0008] Wherein, A includes at least one of a metal element, an inorganic compound or an organic compound, the metal element includes at least one of Li, Na, K, Mg, and Al, the inorganic compound includes NH3 (ammonia), and the organic compound includes PEO (polyethylene oxide);
[0009] M includes at least one of the transition metals Ti, Mo, V, Co, Ni, Zr, Nb, Ta, W, Tc, Rh, Pd, Hf, Re, Tr, and Pt;
[0010] X includes at least one of S, Se, and Te;
[0011] 0.3≤n≤3;
[0012] The two-dimensional layered material comprises a plurality of stacked sheets and a plurality of embedded layers, wherein the embedded layers are located between the sheets;
[0013] The sheet layer includes MX2, and the embedded layer includes A.
[0014] Preferably, A includes at least one of Li, Na and K.
[0015] Preferably, M includes at least one of Ti, Mo, V, Co, Ni, Zr, Nb, Ta, and W.
[0016] Preferably, X includes S.
[0017] Preferably, 0.4≤n≤1.3.
[0018] Preferably, the two-dimensional layered material has a thickness of 50-500 nm, a width of 0.1-5 μm, and an interlayer spacing of 0.55-1.2 nm.
[0019] Preferably, the two-dimensional layered material has a thickness of 120-160 nm, a width of 3.3-4.5 μm, and an interlayer spacing of 0.62-0.72 nm.
[0020] In an embodiment of the present invention, the two-dimensional layered material has high temperature expansion characteristics, and the high temperature expansion characteristics include:
[0021] The initial expansion temperature of two-dimensional layered materials is 150~200℃;
[0022] The volume expansion rate of two-dimensional layered materials is 1000%~2000%;
[0023] and / or,
[0024] The specific surface area of the two-dimensional layered material before expansion is recorded as S2, and the specific surface area of the two-dimensional layered material after full expansion is recorded as S3. S2 and S3 satisfy the following relationship:
[0025] 10≤S3 / S2≤20.
[0026] Preferably, the high temperature expansion properties include:
[0027] The initial expansion temperature of two-dimensional layered materials is 155~180℃;
[0028] The volume expansion rate of two-dimensional layered materials is 1200%~2000%;
[0029] 11≤S3 / S2≤17.
[0030] In a second aspect, the present invention provides a method for preparing the above-mentioned two-dimensional layered material, when A includes a metal element, the preparation method includes using an electrochemical method to embed A between the sheets of the two-dimensional material MX2;
[0031] or,
[0032] When A includes an inorganic compound and / or an organic compound, the preparation method includes using a chemical method to embed A between the sheets of the two-dimensional material MX2.
[0033] In a specific embodiment of the present invention, when A includes a metal element, the preparation method includes the following steps:
[0034] (1) Mixing the two-dimensional material MX2, a first binder and a first solvent to prepare a slurry; coating the slurry on a current collector, drying, rolling and cutting to obtain a pole piece;
[0035] (2) assembling the electrode sheet, metal A, separator and electrolyte prepared in step (1) to obtain a battery;
[0036] (3) discharging the battery prepared in step (2) and obtaining a battery containing the two-dimensional layered material A by controlling the discharge cutoff gram capacity of MX2. n MX2 pole piece;
[0037] (4) using a second solvent to treat the two-dimensional layered material A obtained in step (3) nThe pole piece of MX2 is cleaned to remove the residual first binder and electrolyte, and after drying, a cleaned pole piece is obtained;
[0038] (5) placing the cleaned electrode obtained in step (4) in a third solvent, performing ultrasonic treatment or immersion treatment, filtering the resulting solution to obtain a solid substance; washing and drying the solid substance to obtain a two-dimensional layered material.
[0039] In an embodiment of the present invention, the first binder includes at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), acrylic resin (PAA), styrene-butadiene rubber (SBR), polyetheretherketone (PEEK), polyether block amide (PEBA), polyurethane (TPU), and polyhexamethylene adipamide (PA66).
[0040] In an embodiment of the present invention, the first solvent includes an organic solvent.
[0041] In an embodiment of the present invention, the second solvent includes at least one of N-methylpyrrolidone (NMP) and acetone.
[0042] In an embodiment of the present invention, the third solvent includes at least one of water, alcohols, ketones, and N-methylpyrrolidone (NMP).
[0043] Preferably, in step (3), the discharge cutoff gram capacity of MX2 is 30-750 mAh / g.
[0044] Preferably, in step (5), the power of the ultrasonic treatment is 0-800 W, and the time of the ultrasonic treatment is 0-20 min.
[0045] Preferably, in step (5), the soaking time is 10 to 60 min.
[0046] In a third aspect, the present invention provides a positive electrode sheet, the positive electrode active material layer of the positive electrode sheet includes a positive electrode active material, a conductive agent, a second binder, and the above-mentioned two-dimensional layered material and / or the two-dimensional layered material prepared by the above-mentioned preparation method.
[0047] Preferably, the positive electrode active material includes lithium cobalt oxide material and / or ternary material.
[0048] In the embodiment of the present invention, the molecular formula of the lithium cobalt oxide material is LiCo m T 1-m O2, wherein T includes at least one of Mn, Al, Mg, Ti, Zr, Ca, Fe, and W, and 0.9≤m≤1.0.
[0049] In the embodiment of the present invention, the molecular formula of the ternary material is LiNi x Coy N 1-x-y O2, wherein N includes at least one of Mn, Al, Mg, Ti, Zr, W, and B, 0.4≤x≤1.0, 0≤y≤0.4, and x+y≤1.0.
[0050] In the embodiment of the present invention, the mass percentage of each component in the positive electrode active material layer is:
[0051] Positive electrode active material 90%~99%
[0052] Conductive agent 0.1%~9.8%
[0053] Second binder 0.1%~9.8%
[0054] Two-dimensional layered materials 0.1%~5%.
[0055] In a fourth aspect, the present invention provides a lithium-ion battery comprising the above-mentioned positive electrode sheet.
[0056] Compared with the prior art, the present invention has the following beneficial effects:
[0057] 1. The two-dimensional layered material of the present invention captures oxygen released by the positive electrode material at high temperature (the oxygen capture equation is: MX2+3O2→MO2+2XO2). It can effectively increase the surface area of the reaction at a very low addition amount (≤1wt%), better capture oxygen, and ensure battery safety.
[0058] 2. The two-dimensional layered material of the present invention has a small volume at room temperature, which hardly affects the energy density of the battery and the performance of the battery cell at normal temperature. After the two-dimensional layered material is embedded with A atoms or molecules, the interlayer spacing of the material becomes larger, and it is unstable at high temperatures and will expand. Its surface area can be increased by 10 to 20 times, greatly improving the ability to capture oxygen. Therefore, the required safety effect can be achieved when the two-dimensional layered material is added in a very low amount in the active layer (≤1wt%).
[0059] 3. The expansion temperature of the two-dimensional layered material of the present invention is controllable, and the particle thickness can be reduced to the nanometer level, which is conducive to the adaptation to different positive electrode material systems.
[0060] 4. The two-dimensional layered material of the present invention has good electrical conductivity and has an effect similar to that of graphite conductive agents when used normally. It can be used as a conductive additive to improve the conductivity of the electrode and reduce the internal resistance, which is beneficial to the performance of its electrical properties.
[0061] 5. The two-dimensional layered material of the present invention, in terms of the synthesis method, can, on the one hand, control the molar number of the embedded substance by the discharge capacity, thereby controlling the interlayer distance of the initial two-dimensional material; on the other hand, the material interlayer distance can be further expanded by controlling the type of solvent, as well as the power and time of ultrasound, and the final expansion temperature of the material can be adjusted to prepare materials with different expansion volumes, and can be adapted to different positive electrode material systems to meet the requirements of high-energy systems for larger expansion coefficients. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 This is a schematic diagram of the principle of using expandable two-dimensional layered materials to improve battery safety. The two-dimensional layered material is used as a conductive agent, which expands when the temperature rises, separates and individually wraps the positive electrode active materials, and captures the oxygen released by the positive electrode active materials, thereby inhibiting heat diffusion and improving battery safety.
[0063] Figure 2 This is a schematic diagram of controlling the molar number of intercalated ions by discharge capacity using an electrochemical method. The ordinate is voltage and the abscissa is the molar number of intercalated alkali metals (Li / Na / K, etc.). DETAILED DESCRIPTION
[0064] The present invention discloses a two-dimensional layered material and a method for preparing the same, a positive electrode sheet and a lithium-ion battery. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0065] Terminology explanation:
[0066] Intrinsic safety refers to the safety of the battery itself. Battery intrinsic safety issues mainly include battery short circuit, overcharge, over discharge, overheating and other problems. These problems may lead to safety accidents such as battery explosion and fire, posing a great threat to people's lives and property safety.
[0067] In the description of the present invention, it should be noted that the terms "first", "second", etc. are only used for descriptive purposes, and do not indicate or imply relative importance.
[0068] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.
[0069] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range or the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0070] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0071] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0072] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0073] In order to capture the oxygen released by the active positive electrode material while reducing the impact on the volume of the active material of the battery core, the present invention uses expandable two-dimensional layered materials as conductive agents added to the positive electrode sheet to improve the safety performance of the battery. Specifically, the present invention adopts the following technical solutions:
[0074] In a first aspect, the present invention provides a two-dimensional layered material, the molecular formula of which is A n MX2;
[0075] Wherein, A includes at least one of a metal element, an inorganic compound or an organic compound, the metal element includes at least one of Li, Na, K, Mg, and Al, the inorganic compound includes NH3 (ammonia), and the organic compound includes PEO (polyethylene oxide);
[0076] M includes at least one of the transition metals Ti, Mo, V, Co, Ni, Zr, Nb, Ta, W, Tc, Rh, Pd, Hf, Re, Tr, and Pt;
[0077] X includes at least one of S, Se, and Te;
[0078] 0.3≤n≤3;
[0079] The two-dimensional layered material comprises a plurality of stacked sheets and a plurality of embedded layers, wherein the embedded layers are located between the sheets;
[0080] The sheet layer includes MX2, and the embedded layer includes A.
[0081] In an embodiment of the present invention, when A is a metal element, A is a metal atom and / or a metal ion.
[0082] In an embodiment of the present invention, the number of the sheets is an integer greater than or equal to 2. Exemplarily, the number of the sheets is any value among 2, 5, 10, 15, 20, 25, 30, 40, 50, 100 or any value within the range consisting of any two of the above values.
[0083] In an embodiment of the present invention, the number of embedded layers is an integer greater than or equal to 1, and the number of embedded layers is less than the number of sheet layers. Exemplarily, the number of embedded layers is any value among 1, 4, 9, 14, 19, 24, 29, 39, 49, 99, or any value within the range of any two of the above values.
[0084] Preferably, A includes at least one of Li, Na, and K. The three alkali metals Li, Na, and K can be electrochemically embedded into the two-dimensional material MX2 to increase the interlayer spacing, and the interlayer spacing and expansion degree of the material can be controlled by controlling the amount of embedded alkali metals. Mg and Al have high valence states and are embedded in small amounts; while NH3 and PEO are generally embedded by chemical methods, and have poor controllability.
[0085] Taking cost into comprehensive consideration, M preferably includes at least one of Ti, Mo, V, Co, Ni, Zr, Nb, Ta, and W.
[0086] In a specific embodiment of the present invention, X includes S.
[0087] In the embodiment of the present invention, 0.3≤n≤3. Exemplarily, n is any value among 0.3, 0.4, 0.5, 1.0, 1.3, 1.5, 2.0, 2.5, 3, or any value within the range consisting of any two of the above values.
[0088] Preferably, 0.4≤n≤1.3.
[0089] Preferably, the thickness of the two-dimensional layered material is 50 to 500 nm. Exemplarily, the thickness of the two-dimensional layered material is 50 nm, 52 nm, 55 nm, 60 nm, 65 nm, 80 nm, 100 nm, 120 nm, 130 nm, 140 nm, 148 nm, 150 nm, 155 nm, 160 nm, 180 nm, 200 nm, 300 nm, 400 nm, 500 nm, or any value within the range of any two of the above values.
[0090] Preferably, the thickness of the two-dimensional layered material is 120-160 nm.
[0091] Preferably, the width of the two-dimensional layered material is 0.1-5 μm. Exemplarily, the width of the two-dimensional layered material is any value among 0.1 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.3 μm, 3.5 μm, 3.6 μm, 3.8 μm, 4 μm, 4.1 μm, 4.2 μm, 4.3 μm, 4.5 μm, 5 μm, or any value within the range of any two of the above values.
[0092] Preferably, the width of the two-dimensional layered material is 3.3-4.5 μm.
[0093] Preferably, the interlayer spacing of the two-dimensional layered material is 0.55-1.2 nm. Exemplarily, the interlayer spacing of the two-dimensional layered material is 0.55 nm, 0.58 nm, 0.6 nm, 0.62 nm, 0.65 nm, 0.67 nm, 0.68 nm, 0.7 nm, 0.71 nm, 0.72 nm, 0.8 nm, 0.9 nm, 0.95 nm, 1 nm, 1.1 nm, 1.15 nm, 1.2 nm, or any value in the range of any two of the above values. When the interlayer spacing is greater than 1.2 nm, the two-dimensional layered material will expand into a single-layer material in advance, causing the electronic conductivity of the material to deteriorate, and the ability to expand at high temperature will be lost, and safety cannot be effectively improved.
[0094] Preferably, the interlayer spacing of the two-dimensional layered material is 0.62-0.72 nm.
[0095] In an embodiment of the present invention, the two-dimensional layered material has high temperature expansion characteristics, and the high temperature expansion characteristics include:
[0096] The initial expansion temperature of two-dimensional layered materials is 150~200℃;
[0097] The volume expansion rate of two-dimensional layered materials is 1000%~2000%;
[0098] and / or,
[0099] The specific surface area of the two-dimensional layered material before expansion is recorded as S2, and the specific surface area of the two-dimensional layered material after full expansion is recorded as S3. S2 and S3 satisfy the following relationship:
[0100] 10≤S3 / S2≤20.
[0101] Exemplarily, the initial expansion temperature of the two-dimensional layered material is any value among 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C, or any value within the range consisting of any two of the above values.
[0102] Exemplarily, the volume expansion rate of the two-dimensional layered material is any value of 1000%, 1100%, 1200%, 1300%, 1400%, 1500%, 1600%, 1700%, 1800%, 1900%, 2000%, or any value within the range consisting of any two of the above values.
[0103] Exemplarily, the ratio of S3 / S2 is any value among 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 or any value within the range consisting of any two of the above values.
[0104] Preferably, the high temperature expansion properties include:
[0105] The initial expansion temperature of two-dimensional layered materials is 155~180℃;
[0106] The volume expansion rate of two-dimensional layered materials is 1200%~2000%;
[0107] 11≤S3 / S2≤17.
[0108] In a second aspect, the present invention provides a method for preparing the above-mentioned two-dimensional layered material, when A includes a metal element, the preparation method includes using an electrochemical method to embed A between the sheets of the two-dimensional material MX2;
[0109] or,
[0110] When A includes an inorganic compound and / or an organic compound, the preparation method includes using a chemical method to embed A between the sheets of the two-dimensional material MX2.
[0111] In a specific embodiment of the present invention, when A includes a metal element, the preparation method includes the following steps:
[0112] (1) Mixing the two-dimensional material MX2, a first binder and a first solvent to prepare a slurry; coating the slurry on a current collector, drying, rolling and cutting to obtain a pole piece;
[0113] (2) assembling the electrode sheet, metal A, separator and electrolyte prepared in step (1) to obtain a battery;
[0114] (3) discharging the battery prepared in step (2) and obtaining a battery containing the two-dimensional layered material A by controlling the discharge cutoff gram capacity of MX2. n MX2 pole piece;
[0115] (4) using a second solvent to treat the two-dimensional layered material A obtained in step (3) n The pole piece of MX2 is cleaned to remove the residual first binder and electrolyte, and after drying, a cleaned pole piece is obtained;
[0116] (5) placing the cleaned electrode obtained in step (4) in a third solvent, performing ultrasonic treatment or immersion treatment, filtering the resulting solution to obtain a solid substance; washing and drying the solid substance to obtain a two-dimensional layered material.
[0117] In the present invention, when A includes inorganic compounds and / or organic compounds, the method for preparing the two-dimensional layered material includes using a chemical method to embed A between the sheets of the two-dimensional material MX2. The present invention can adopt conventional chemical methods as long as the purpose of the present invention can be achieved. Exemplarily, when A includes inorganic compounds and / or organic compounds, the method for preparing the two-dimensional layered material includes: placing the two-dimensional material MX2 in a solution containing A (the mass concentration of A is preferably 10% to 60%) for ultrasonic treatment, the power of the ultrasonic treatment is preferably 500 to 800 W, and the time of the ultrasonic treatment is preferably 1 to 5 h. The sonicated solution is then centrifuged. The obtained supernatant is mixed with an appropriate amount of water (for example, a volume ratio of 1: 0.1 to 1), allowed to stand for 4 to 10 minutes, and dried to obtain a two-dimensional layered material A. n MX2.
[0118] In an embodiment of the present invention, the size of the two-dimensional material MX2 is 1 to 1000 μm. Exemplarily, the size of the two-dimensional material MX2 is any value among 1 μm, 5 μm, 10 μm, 50 μm, 100 μm, 200 μm, 400 μm, 500 μm, 600 μm, 800 μm, 1000 μm, or any value within the range of any two of the above values. Preferably, it is 5 to 100 μm.
[0119] In an embodiment of the present invention, the first binder includes at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), acrylic resin (PAA), styrene-butadiene rubber (SBR), polyetheretherketone (PEEK), polyether block amide (PEBA), polyurethane (TPU), and polyhexamethylene adipamide (PA66). Polyvinylidene fluoride (PVDF) is preferred.
[0120] In an embodiment of the present invention, the first solvent includes an organic solvent.
[0121] Preferably, the first solvent includes but is not limited to N-methylpyrrolidone (NMP);
[0122] In an embodiment of the present invention, the second solvent includes at least one of N-methylpyrrolidone (NMP) and acetone.
[0123] Preferably, the second solvent is NMP, which can dissolve the first binder more effectively. When the second solvent is acetone, it needs to be properly heated (40-100° C.) to better dissolve the first binder.
[0124] In an embodiment of the present invention, the third solvent includes at least one of water, alcohols, ketones, and N-methylpyrrolidone (NMP), preferably water, such as deionized water.
[0125] Preferably, in step (3), the discharge cut-off gram capacity of MX2 is 30-750 mAh / g. Exemplarily, the discharge cut-off gram capacity of MX2 is any value of 30 mAh / g, 50 mAh / g, 80 mAh / g, 90 mAh / g, 100 mAh / g, 200 mAh / g, 220 mAh / g, 240 mAh / g, 300 mAh / g, 400 mAh / g, 500 mAh / g, 600 mAh / g, 700 mAh / g, 750 mAh / g, or any value within the range of any two of the above values.
[0126] Preferably, the discharge cut-off gram capacity of MX2 is 80-240 mAh / g.
[0127] Two-dimensional layered material A n The A atom in MX2 reacts with the third solvent to produce gases such as H2. The generated gas further increases the interlayer spacing, which is beneficial to the later expansion of the material.
[0128] Exemplarily, the reaction equation of lithium atoms in water is:
[0129] Li+H2O→LiOH+1 / 2H2↑;
[0130] Exemplarily, the reaction equation of lithium atoms in ethanol is:
[0131] Li+CH3CH2OH→CH3CH2OLi+1 / 2H2↑.
[0132] Exemplarily, the reaction equation of sodium atom in ethanol is:
[0133] Na+CH3CH2OH→CH3CH2ONa+1 / 2H2↑.
[0134] Because sodium or potassium reacts more violently with water, when A is Na or K, the third solvent is preferably a mild alcohol, such as ethanol, and the time of ultrasonic treatment can be appropriately increased.
[0135] In an embodiment of the present invention, the role of ultrasonic treatment is to accelerate the reaction of A atom and the third solvent.
[0136] Preferably, in step (5), the power of ultrasonic treatment is 0-800 W, and the time of ultrasonic treatment is 0-20 min. Exemplarily, the power of ultrasonic treatment is any value in 0.1 W, 1 W, 10 W, 100 W, 200 W, 300 W, 400 W, 500 W, 600 W, 700 W, 800 W, or any value in the range of any two of the above values. Exemplarily, the time of ultrasonic treatment is any value in 0.1 min, 1 min, 2 min, 4 min, 6 min, 8 min, 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, or any value in the range of any two of the above values. The power of ultrasonic treatment is greater than 800 W, and / or the time of ultrasonic treatment is greater than 20 min, which will cause the material to peel off and expand prematurely, which is not conducive to dispersion after becoming nanoparticles, and the expected safety effect cannot be achieved in the battery.
[0137] Preferably, in step (5), the power of the ultrasonic treatment is 400-600 W, and the time of the ultrasonic treatment is 2-5 min.
[0138] Preferably, in step (5), the soaking time is 10 to 60 min. Exemplarily, the soaking time is any one of 10 min, 20 min, 30 min, 40 min, 50 min, and 60 min, or any value within the range of any two of the above values.
[0139] In a third aspect, the present invention provides a positive electrode sheet, the positive electrode active material layer of the positive electrode sheet includes a positive electrode active material, a conductive agent, a second binder, and the above-mentioned two-dimensional layered material and / or the two-dimensional layered material prepared by the above-mentioned preparation method.
[0140] Preferably, the positive electrode active material includes lithium cobalt oxide material and / or ternary material.
[0141] In the embodiment of the present invention, the molecular formula of the lithium cobalt oxide material is LiCo m T 1-m O2, wherein T includes at least one of Mn, Al, Mg, Ti, Zr, Ca, Fe, and W, and 0.9≤m≤1.0. Exemplarily, the molecular formula of the lithium cobalt oxide material is LiCo 0.9 Mn 0.1 O2、LiCo 0.95 Mn 0.05 O2, LiCoO2, etc.
[0142] In the embodiment of the present invention, the molecular formula of the ternary material is LiNi x Co y N 1-x-y O2, wherein N includes at least one of Mn, Al, Mg, Ti, Zr, W, and B, 0.4≤x≤1.0, 0≤y≤0.4, and x+y≤1.0. Exemplarily, the molecular formula of the ternary material is LiNi 0.4 Co 0.4 Mn 0.2 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.9 Co 0.1 O2, LiNiO2, etc.
[0143] In the embodiment of the present invention, the mass percentage of each component in the positive electrode active material layer is:
[0144] Positive electrode active material 90%~99%
[0145] Conductive agent 0.1%~9.8%
[0146] Second binder 0.1%~9.8%
[0147] Two-dimensional layered materials 0.1%~5%.
[0148] Exemplarily, the mass ratio of the positive electrode active material, the two-dimensional layered material, the conductive agent and the second binder is 95:1:2:2, 90:5:2.5:2.5, 99:0.1:0.45:0.45, etc. In the embodiment of the present invention, when the proportion of the two-dimensional layered material is greater than 5%, it will cause a large capacity loss; when the proportion of the two-dimensional layered material is less than 0.1%, it is difficult to play a role in improving safety.
[0149] In the embodiment of the present invention, the conductive agent includes but is not limited to at least one of conductive graphite, conductive carbon black (such as conductive carbon black SP), conductive carbon fiber, carbon nanotube or graphene. In addition to the several specific substances listed above, other types of conductive agents recognized by those skilled in the art are within the protection scope of the present invention.
[0150] In the embodiment of the present invention, the second binder is but not limited to at least one of polyvinylidene fluoride (PVDF), styrene butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC), polyacrylate (LA), and polyacrylic acid binder (PAA). In addition to the several specific substances listed above, other types of binders recognized by those skilled in the art are within the scope of protection of the present invention.
[0151] The present application has no particular restrictions on the preparation method of the positive electrode sheet. Those skilled in the art can prepare the positive electrode sheet according to conventional preparation methods as long as the purpose of the present application can be achieved. Exemplarily, the preparation method of the positive electrode sheet includes: mixing the positive electrode active material, the conductive agent, the second binder and the two-dimensional layered material uniformly, adding a solvent to prepare a positive electrode slurry; coating the positive electrode slurry on the positive electrode current collector, and obtaining the positive electrode sheet after drying.
[0152] In a fourth aspect, the present invention provides a lithium-ion battery comprising the above-mentioned positive electrode sheet.
[0153] In the embodiment of the present invention, the battery structure includes but is not limited to button batteries, soft-pack batteries, cylindrical batteries, etc.
[0154] The present application has no particular restrictions on the negative electrode sheet, separator, and electrolyte in the battery, and those skilled in the art can select them according to actual needs as long as the purpose of the present application can be achieved.
[0155] The reagents, instruments or materials used in the present invention can be obtained through commercial channels.
[0156] The present invention will be further described below in conjunction with embodiments:
[0157] Embodiment 1:
[0158] 1. Preparation of two-dimensional layered materials
[0159] This embodiment uses LiTiS2 material as an expandable two-dimensional layered material, and its preparation process is as follows:
[0160] (1) Weigh 95 g of micron-sized TiS2 material (initial material MX2) and 5 g of PVDF (Solvay 5130), mix them in 100 g of NMP (dimethylpyrrolidone) solvent, and then coat the slurry on copper foil. After drying, rolling and cutting, the electrode is prepared.
[0161] (2) The electrode was assembled with a metal lithium foil (50 μm thick) into a battery. The thickness of the separator was 20 μm, the electrolyte was 1.0 M LiPF6, and the solvent was EC / EMC = 3:7 (EC is ethylene carbonate, EMC is ethyl methyl carbonate).
[0162] (3) The assembled battery is discharged at a current of 450 mA (~0.02C rate) (since no additional conductive agent is added during the electrode preparation process, a small current discharge is required to reduce polarization and allow lithium atoms to be embedded in the material), and the discharge cut-off capacity is controlled (e.g. Figure 2 As shown in the figure), the discharge was stopped when it reached 22.7Ah (corresponding to the embedding of 1 mol Li, the discharge cut-off capacity was 22.7Ah, and the corresponding discharge cut-off capacity was 238.9 mAh / g). The molecular formula of the obtained material was LiTiS2.
[0163] (4) Disassemble the discharged battery, clean the electrode sheet with NMP to remove the residual electrolyte and binder, and then dry it.
[0164] (5) The dried electrode was placed in deionized water for ultrasonic treatment at a power of 500 W for 2 min. The material in the solution was filtered, washed and dried to obtain an expandable two-dimensional layered material LiTiS2 (expandable two-dimensional layered material A). n MX2), which has a width of 4.2μm, a thickness of 150nm, and an interlayer spacing of approximately 0.65nm.
[0165] 2. Battery assembly
[0166] (1) The positive electrode active material NCM811, the two-dimensional layered material LiTiS2, the conductive agent SP65, and the binder PVDF5130 were prepared into a positive electrode sheet in a mass ratio of 95:1:2:2.
[0167] (2) The negative electrode active material artificial graphite QC8, the conductive agent SP65, and the binder PVDF5130 are prepared into a negative electrode sheet in a ratio of 95:2:3.
[0168] (3) Assemble the positive electrode, separator, and negative electrode into a lithium-ion battery with a capacity of 20Ah.
[0169] Embodiment 2:
[0170] 1. Preparation of two-dimensional layered materials
[0171] This embodiment uses Li 1.3 MoS2 material is an expandable two-dimensional layered material, and its preparation process is as follows:
[0172] (1) Weigh 95 g of micron-sized MoS2 material (initial material MX2) and 5 g of PVDF (Solvay 5130), mix them in 100 g of NMP solvent, and then coat the slurry on copper foil. After drying, rolling and cutting, the electrode is prepared.
[0173] (2) The electrode was assembled with a metal lithium foil (50 μm thick) into a battery. The thickness of the separator was 20 μm, the electrolyte was 1.0 M LiPF6, and the solvent was EC / EMC = 3:7.
[0174] (3) The assembled battery was discharged at a rate of 0.02C, and the discharge cut-off capacity was controlled. The discharge was stopped when it reached 20.6Ah (corresponding to 1.3 mol Li embedded, a discharge cut-off capacity of 20.6Ah, and a corresponding discharge cut-off capacity of 216.8mAh / g). The molecular formula of the obtained material is Li 1.3 MoS2.
[0175] (4) Disassemble the discharged battery, clean the electrode sheet with NMP to remove the residual electrolyte and binder, and then dry it.
[0176] (5) The dried electrode was placed in deionized water for ultrasonic treatment at a power of 500 W for 2 min. The material in the solution was filtered, washed and dried to obtain an expandable two-dimensional layered material Li 1.3 MoS2 (Expandable 2D Layered Material A n MX2), which has a width of 3.3μm, a thickness of 120nm, and an interlayer spacing of approximately 0.72nm.
[0177] 2. Battery assembly
[0178] Same as Example 1.
[0179] Embodiment 3:
[0180] 1. Preparation of two-dimensional layered materials
[0181] This embodiment uses Na 0.5 MoS2 material is an expandable two-dimensional layered material, and its preparation process is as follows:
[0182] (1) Weigh 95 g of micron-sized MoS2 material (initial material MX2) and 5 g of PVDF (Solvay 5130), mix them in 100 g of NMP solvent, and then coat the slurry on copper foil. After drying, rolling and cutting, the electrode is prepared.
[0183] (2) The electrode was assembled with a sodium foil (50 μm thick) into a battery. The thickness of the separator was 20 μm. The electrolyte was 1.0 M NaPF6 and the solvent was EC / EMC = 3:7.
[0184] (3) The assembled battery was discharged at a rate of 0.01C, and the discharge cut-off capacity was controlled. The discharge was stopped when it reached 7.9Ah (corresponding to 0.5 mol Na embedded, a discharge cut-off capacity of 7.9Ah, and a discharge cut-off capacity of 83.2mAh / g). The molecular formula of the obtained material was Na 0.5 MoS2.
[0185] (4) Disassemble the discharged battery, clean the electrode sheet with NMP to remove the residual electrolyte and binder, and then dry it.
[0186] (5) The dried electrode was placed in ethanol and ultrasonicated for 5 min at a power of 500 W. The material in the solution was filtered, washed and dried to obtain an expandable two-dimensional layered material Na 0.5 MoS2 (Expandable 2D Layered Material A n MX2), which has a width of 3.5μm, a thickness of 130nm, and an interlayer spacing of approximately 0.70nm.
[0187] 2. Battery assembly
[0188] Same as Example 1.
[0189] Embodiment 4:
[0190] 1. Preparation of two-dimensional layered materials
[0191] This embodiment uses K 0.4 TiS2 material is an expandable two-dimensional layered material, and its preparation process is as follows:
[0192] (1) Weigh 95 g of micron-sized TiS2 material (initial material MX2) and 5 g of PVDF (Solvay 5130), mix them in 100 g of NMP solvent, and then coat the slurry on copper foil. After drying, rolling and cutting, the electrode is prepared.
[0193] (2) The electrode was assembled with a metal potassium foil (50 μm thick) into a battery. The thickness of the separator was 20 μm, the electrolyte was 1.0 M KPF6, and the solvent was EC / EMC = 3:7.
[0194] (3) The assembled battery was discharged at a rate of 0.01C, and the discharge cut-off capacity was controlled. The discharge was stopped when it reached 9.0Ah (corresponding to the embedding of 0.4 mol K, the discharge cut-off capacity was 9.0Ah, and the corresponding discharge cut-off capacity was 94.7mAh / g). The molecular formula of the obtained material was K 0.4 TiS2.
[0195] (4) Disassemble the discharged battery, clean the electrode sheet with NMP to remove the residual electrolyte and binder, and then dry it.
[0196] (5) The dried electrode was placed in ethanol and ultrasonicated for 5 min at a power of 500 W. The material in the solution was filtered, washed and dried to obtain an expandable two-dimensional layered material K 0.4 TiS2 (Expandable Two-Dimensional Layered Material A n MX2), which has a width of 4.5μm, a thickness of 160nm, and an interlayer spacing of approximately 0.62nm.
[0197] 2. Battery assembly
[0198] Same as Example 1.
[0199] Example 5a:
[0200] This example is prepared by referring to Example 1, except that:
[0201] When the discharge reaches 6.8Ah in step (3), the discharge is stopped (corresponding to 0.3 mol Li embedded and the discharge cut-off capacity is 71.7 mAh / g). The molecular formula of the obtained material is Li 0.3 TiS2.
[0202] In step (5), the ultrasonic power is 100 W and the time is 20 min.
[0203] Obtain expandable two-dimensional layered material Li 0.3 TiS2, with a width of 5μm, a thickness of 500nm, and an interlayer spacing of approximately 0.58nm.
[0204] Example 5b:
[0205] This example is prepared by referring to Example 1, except that:
[0206] When the discharge reaches 68.1 Ah in step (3), the discharge is stopped (corresponding to 3 mol Li embedded, and the discharge cut-off capacity is 716.7 mAh / g). The molecular formula of the obtained material is Li3TiS2.
[0207] In step (5), the ultrasonic power is 800 W and the time is 1 min.
[0208] The result is an expandable two-dimensional layered material Li3TiS2 with a width of 0.1 μm, a thickness of 140 nm, and an interlayer spacing of approximately 1.2 nm.
[0209] Example 6a:
[0210] This example is prepared by referring to Example 1, except that:
[0211] Obtaining expandable two-dimensional layered material Mg 0.5NbSe2, in step (1), NbSe2 is used as the initial material, in step (2), metal Mg foil is used as the negative electrode, the electrolyte is 1.0M Mg(PF6)2, in step (3), the discharge cut-off capacity is controlled, and the discharge is stopped when it reaches 5.05Ah (corresponding to embedding 0.5mol Mg, the discharge cut-off capacity is 5.05Ah, and the corresponding discharge cut-off capacity is 53.35mAh / g), and the molecular formula of the obtained material is Mg 0.5 In step (5), the material is placed in ethanol and ultrasonicated at a power of 500 W for 5 min to obtain an expandable two-dimensional material Mg 0.5 NbSe2. Its width is 3.8μm, thickness is 50nm, and the interlayer spacing is about 0.68nm.
[0212] Example 6b:
[0213] This example is prepared by referring to Example 1, except that:
[0214] Obtain expandable two-dimensional layered material Al 0.3 CoTe2. In step (1), CoTe2 is used as the initial material, in step (2), metal Al foil is used as the negative electrode, the electrolyte is 1.0M Al(PF6)3, and in step (3), the discharge cut-off capacity is controlled to stop discharging when it reaches 2.43Ah (corresponding to embedding 0.3mol Al, the discharge cut-off capacity is 2.43Ah, and the corresponding discharge cut-off gram capacity is 25.6mAh / g). The molecular formula of the obtained material is Al 0.3 In step (5), the material is placed in ethanol and ultrasonicated at a power of 500 W for 5 min to obtain an expandable two-dimensional material Al 0.3 CoTe2. Its width is 4.1μm, thickness is 65nm, and the interlayer spacing is about 0.70nm.
[0215] Example 6c:
[0216] This example is prepared by referring to Example 1, except that:
[0217] The expandable two-dimensional layered material LiVS2 is obtained. VS2 is used as the initial material in step (1), and the discharge cut-off capacity is controlled in step (3), and the discharge is stopped when it reaches 22.15Ah (corresponding to 1.0 mol Li embedded, the discharge cut-off capacity is 22.15Ah, and the corresponding discharge cut-off gram capacity is 233.2mAh / g). The molecular formula of the obtained material is LiVS2. In step (5), the material is placed in deionized water for ultrasonic treatment with a power of 500W and a time of 5min to obtain the expandable two-dimensional material LiVS2. Its width is 4.3μm, thickness is 155nm, and the interlayer spacing is about 0.67nm.
[0218] Embodiment 6d:
[0219] This example is prepared by referring to Example 1, except that:
[0220] The expandable two-dimensional layered material LiWS2 is obtained. WS2 is used as the initial material in step (1), and the discharge cut-off capacity is controlled in step (3), and the discharge is stopped when it reaches 10.25Ah (corresponding to 1.0 mol Li embedded, the discharge cut-off capacity is 10.25Ah, and the corresponding discharge cut-off gram capacity is 107.9mAh / g). The molecular formula of the obtained material is LiWS2. In step (5), the material is placed in deionized water for ultrasonic treatment with a power of 500W and a time of 5min to obtain the expandable two-dimensional material LiWS2. Its width is 4.5μm, thickness is 148nm, and the interlayer spacing is about 0.71nm.
[0221] Example 7a:
[0222] This example uses a chemical method to prepare expandable two-dimensional material (NH3) n MoS2, the main process is as follows: Take 10g of the initial material MoS2, and perform ultrasonic treatment in 250ml of ammonia solution (25wt%), with an ultrasonic power of 700W and a time of 3h. The solution after ultrasonic treatment is transferred to a centrifuge tube for centrifugation at a speed of 2000rpm for 2min. Then take the supernatant and soak it in deionized water for 5min, and then dry it to obtain the expandable two-dimensional material (NH3) n MoS2 (chemical methods have poor controllability, considering that NH3 molecules are large, usually 0.3≤n<0.5), with a width of 3.6μm, a thickness of 55nm, and an interlayer spacing of about 0.95nm.
[0223] Example 7b:
[0224] This example uses a chemical method to prepare an expandable two-dimensional material (PEO) n MoS2, its main process is as follows: take 10g of the initial material MoS2, and perform ultrasonic treatment in 500ml of PEO aqueous solution (the mass ratio of PEO to water is 1:1), the ultrasonic power is 700W, and the time is 3h. The solution after ultrasonic treatment is transferred to a centrifuge tube for centrifugal treatment at a speed of 2000rpm for 2min. Then take the supernatant and soak it in deionized water for 5min, and then dry it to obtain the expandable two-dimensional material (PEO) n MoS2 (chemical methods have poor controllability, considering that PEO molecules are large, usually 0.3≤n<0.5) has a width of 3.5μm, a thickness of 52nm, and an interlayer spacing of about 1.15nm.
[0225] Example 8a:
[0226] This example is prepared by referring to Example 1, except that:
[0227] (5) Soak the dried electrode in deionized water for 10 min. Filter the material in the solution, wash it, and dry it to obtain expandable two-dimensional layered material LiTiS2 (expandable two-dimensional layered material A). n MX2), which has a width of 4.2μm, a thickness of 150nm, and an interlayer spacing of approximately 0.65nm.
[0228] Example 8b:
[0229] This example is prepared by referring to Example 1, except that:
[0230] (5) The dried electrode was placed in deionized water for 60 minutes. The material in the solution was filtered, washed and dried to obtain expandable two-dimensional layered material LiTiS2 (expandable two-dimensional layered material A). n MX2), which has a width of 4.2μm, a thickness of 150nm, and an interlayer spacing of approximately 0.65nm.
[0231] Comparative Example 1:
[0232] In this comparative example, the positive electrode sheet is not added with expandable two-dimensional layered material, and when the battery is manufactured, the active positive electrode material NCM811, the conductive agent SP65, and the binder PVDF5130 are prepared into a positive electrode sheet in a ratio of 96:2:2. Others are the same as in Example 1.
[0233] Comparative Example 2a:
[0234] This comparative example uses Li 0.2 TiS2 material is an expandable two-dimensional layered material with less embedded lithium ions. Its preparation process is similar to that of Example 1, except that the discharge cut-off capacity is controlled and the discharge is stopped when it reaches 4.5Ah (corresponding to embedding 0.2mol Li, the discharge cut-off capacity is 4.5Ah, and the corresponding discharge cut-off capacity is 47.8 mAh / g). The molecular formula of the obtained material is Li 0.2 TiS2 (Expandable Two-Dimensional Layered Material A n MX2), which has a width of 4.8μm, a thickness of 300nm, and an interlayer spacing of approximately 0.59nm.
[0235] Comparative Example 2b:
[0236] This comparative example uses Li 3.2TiS2 material is an expandable two-dimensional layered material with more embedded lithium ions. Its preparation process is similar to that of Example 1, except that the discharge cut-off capacity is controlled and the discharge is stopped when it reaches 72.6Ah (corresponding to 3.2 mol Li embedded, the discharge cut-off capacity is 72.6Ah, and the corresponding discharge cut-off capacity is 764.5 mAh / g). The molecular formula of the obtained material is Li 3.2 TiS2 (Expandable Two-Dimensional Layered Material A n MX2), which has a width of 0.12μm, a thickness of 2.8nm, and an interlayer spacing of approximately 0.57nm.
[0237] Comparative Example 3a:
[0238] This comparative example uses LiTiS2 material as an expandable two-dimensional layered material, and its preparation process is similar to that of Example 1. The discharge is stopped when it reaches 22.7Ah (corresponding to embedding 1 mol Li, the discharge cut-off capacity is 22.7Ah, and the corresponding discharge cut-off gram capacity is 238.9mAh / g). The molecular formula of the obtained material is LiTiS2. The difference is that the ultrasonic power is 1200W (the ultrasonic power is too large, exceeding 800W), the ultrasonic time is 30min (the ultrasonic time is too long, exceeding 20min), and the width of the material expanded in advance is 4.2μm, the thickness is 2.6nm, and the interlayer spacing is about 0.57nm.
[0239] Comparative Example 3b:
[0240] This comparative example uses LiTiS2 material as an expandable two-dimensional layered material, and its preparation process is similar to that of Example 1. The discharge is stopped when it reaches 22.7Ah (corresponding to embedding 1 mol Li, the discharge cut-off capacity is 22.7Ah, and the corresponding discharge cut-off gram capacity is 238.9 mAh / g). The molecular formula of the obtained material is LiTiS2. The difference is that the ultrasonic power is 900W (the ultrasonic power is too large, exceeding 800W), the ultrasonic time is 21min (the ultrasonic time is too long, exceeding 20min), and the width of the material expanded in advance is 4.3μm, the thickness is 3.0nm, and the interlayer spacing is about 0.57nm.
[0241] Test Example 1
[0242] The performance of the two-dimensional layered materials and batteries prepared in the above examples and comparative examples was tested:
[0243] (1) Expansion temperature and volume expansion rate
[0244] Test the expansion volume of the expandable two-dimensional layered material. Take 2g of the expandable two-dimensional layered material A nMX2 is placed in a container, and its volume V1 is read. In an inert environment (N2), the temperature is raised to 350°C at a rate of 5°C / min (the temperature of thermal runaway of lithium-ion batteries is generally below 300°C, usually between 200-300°C. Expandable two-dimensional layered materials are preferably expanded before 200°C). The temperature at which expansion begins is recorded, and the final expansion material (recorded as pA) is read. n MX2) volume V2, calculate the volume expansion ratio V2 / V1.
[0245] (2) Specific surface area
[0246] The specific surface areas of three materials were tested, referring to GB / T 19587-2017 "Determination of specific surface area of solid substances by gas adsorption BET method". One is the initial micron-level MX2 (S1), and the other is A after the reaction is completed. n MX2 (S2), one is pA after expansion n MX2(S3).
[0247] (3) Proportion of oxygen captured at 200°C
[0248] Weigh 5 g of material, pass 0.3 mol of oxygen into it, heat it to 200°C in a 100 mL sealed container, then stop heating, and test the remaining oxygen content when it cools naturally to room temperature, and calculate the proportion of captured oxygen.
[0249] (4) Diaphragm resistance
[0250] The film resistance of the positive electrode is measured using Yuanneng Technology's electrode resistance meter.
[0251] (5) Discharge capacity and gram capacity
[0252] The battery was charged and discharged between 2.7 and 4.2 V to test its capacity (charging at 1C constant current and constant voltage, with a cut-off current of 0.05C; discharging at 1C), and the gram capacity of the positive electrode material was calculated.
[0253] (6) Cycle test
[0254] The cycle test refers to GB / T 31484-2015, the charging mode is 1C constant current and constant voltage, the cut-off current in the constant voltage stage is 0.05C; the discharge is 1C. The capacity retention rate after 100 cycles is tested.
[0255] (7) DC internal resistance
[0256] The battery was discharged to 50% SOC (state of charge) and discharged at 4C for 10s to test its DC internal resistance.
[0257] (8) Acupuncture safety test
[0258] The 4.2V full charge needle puncture safety test is carried out in accordance with the national standard GB / T 31485-2015.
[0259] The test results are shown in Table 1 and Table 2.
[0260] Table 1 shows the material properties of the embodiments and comparative examples, including the size, expansion temperature, volume expansion rate, specific surface area before and after expansion, and the proportion of oxygen captured at 200° C. of the expandable two-dimensional layered material;
[0261] Table 2 shows the battery characteristics of the embodiments and comparative examples, including positive electrode sheet resistance, gram capacity of positive electrode active material, discharge capacity, capacity retention rate after 100 cycles, battery internal resistance, and puncture safety.
[0262]
[0263]
[0264] The above results show that by controlling the discharge capacity of different materials, the number of moles of alkali metals embedded in the material can be accurately controlled to prepare a two-dimensional layered material with specific parameters. Then, its expansion temperature (generally less than 200°C) is controlled so that it expands and increases in volume before the positive active material is decomposed and releases oxygen (generally above 200°C) when it is at a high temperature to prevent thermal runaway and improve the safety of the battery cell. After adding the two-dimensional layered material of the present invention to the electrode sheet, Examples 1 to 8 can ensure the safety of acupuncture, and the two-dimensional layered material has good electronic conductivity, so the resistance of the prepared positive electrode sheet is reduced, the gram capacity of the positive electrode material is increased, and the discharge internal resistance of the battery is relatively low, and the cycle life is better than the control example, which has no effect on the electrical performance as a whole.
[0265] Comparative Example 1 did not add expandable two-dimensional layered materials, could not pass the needle puncture test, and the battery safety could not be improved.
[0266] In Comparative Example 2a, the degree of lithium insertion is too low, the material expansion temperature exceeds 300°C, the increase in volume and surface area after expansion is not obvious, and it cannot pass the needle puncture test, and the battery safety cannot be improved.
[0267] In Comparative Example 2b, the degree of lithium insertion is too high and the increase in interlayer spacing is too large. When it exceeds the constraint capacity of the van der Waals force of the material itself, it will cause the material to expand prematurely. The volume and surface area of the subsequent electrode will basically not change much, and the battery safety cannot be improved.
[0268] In comparative example 3, the ultrasonic power exceeded 800W and the time exceeded 20 minutes, which caused the material to expand prematurely. The volume and surface area of the subsequent electrode sheet were basically unchanged, and the battery safety could not be improved. Moreover, the electronic conductivity of the material that expanded prematurely decreased, resulting in an increase in the resistance of the positive electrode sheet, a decrease in the positive electrode capacity, an increase in the internal resistance of the battery, and poor circulation. Not only did it fail the needle puncture test, but it also affected the performance of the battery.
[0269] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A two-dimensional layered material, characterized in that: The molecular formula of the two-dimensional layered material is A n MX2; Wherein, A comprises at least one of a metal element, an inorganic compound or an organic compound, the metal element comprises at least one of Li, Na, K, Mg and Al, the inorganic compound comprises NH3, and the organic compound comprises PEO; M includes at least one of the transition metals Ti, Mo, V, Co, Ni, Zr, Nb, Ta, W, Tc, Rh, Pd, Hf, Re, Tr, and Pt; X includes at least one of S, Se, and Te; 0.3≤n≤3; The two-dimensional layered material comprises a plurality of stacked sheets and a plurality of embedded layers, wherein the embedded layers are located between the sheets; The sheet layer includes MX2, and the embedded layer includes A; The two-dimensional layered material has high temperature expansion characteristics, and the high temperature expansion characteristics include: The initial expansion temperature of the two-dimensional layered material is 150-200°C; The volume expansion rate of the two-dimensional layered material is 1000% to 2000%.
2. The two-dimensional layered material according to claim 1, characterized in that The A includes at least one of Li, Na, and K; The M includes at least one of Ti, Mo, V, Co, Ni, Zr, Nb, Ta, and W; Said X includes S; 0.4≤n≤1.3。 3. The two-dimensional layered material according to claim 1, characterized in that The two-dimensional layered material has a thickness of 50-500 nm, a width of 0.1-5 μm, and an interlayer spacing of 0.55-1.2 nm.
4. The two-dimensional layered material according to any one of claims 1 to 3, characterized in that The specific surface area of the two-dimensional layered material before expansion is recorded as S2, and the specific surface area of the two-dimensional layered material after full expansion is recorded as S3. S2 and S3 satisfy the following relationship: 10≤S3 / S2≤20.
5. A method for preparing the two-dimensional layered material according to any one of claims 1 to 4, characterized in that: When A includes a metal element, the preparation method includes embedding A between the sheets of the two-dimensional material MX2 using an electrochemical method; or, When A comprises an inorganic compound and / or an organic compound, the preparation method comprises embedding A between the sheets of the two-dimensional material MX2 by a chemical method.
6. The preparation method according to claim 5, characterized in that: When A includes a metal element, the preparation method comprises the following steps: (1) Mixing a two-dimensional material MX2, a first binder, and a first solvent to prepare a slurry; coating the slurry on a current collector, drying, rolling, and cutting to obtain a pole piece; (2) assembling the electrode sheet, metal A, separator and electrolyte prepared in step (1) to obtain a battery; (3) discharging the battery prepared in step (2) and obtaining a battery containing the two-dimensional layered material A by controlling the discharge cutoff gram capacity of MX2. n MX2 pole piece; (4) using a second solvent to treat the two-dimensional layered material A obtained in step (3) n The pole piece of MX2 is cleaned to remove the residual first binder and electrolyte, and after drying, a cleaned pole piece is obtained; (5) placing the cleaned electrode obtained in step (4) in a third solvent, performing ultrasonic treatment or immersion treatment, filtering the obtained solution to obtain a solid substance; washing and drying the solid substance to obtain a two-dimensional layered material.
7. The preparation method according to claim 6, characterized in that: The first binder includes at least one of polyvinylidene fluoride, polytetrafluoroethylene, acrylic resin, styrene-butadiene rubber, polyetheretherketone, polyether block amide, polyurethane, and polyhexamethylene adipamide; The first solvent comprises an organic solvent; The second solvent includes at least one of N-methylpyrrolidone and acetone; The third solvent includes at least one of water, alcohols, ketones, and N-methylpyrrolidone.
8. The preparation method according to claim 6, characterized in that: In step (3), the discharge cut-off capacity of MX2 is 30-750 mAh / g; In step (5), the power of the ultrasonic treatment is 0 to 800 W, and the time of the ultrasonic treatment is 0 to 20 min; In step (5), the soaking treatment time is 10 to 60 minutes.
9. A positive electrode sheet, characterized in that: The positive electrode active material layer of the positive electrode sheet comprises a positive electrode active material, a conductive agent, a second binder, and the two-dimensional layered material according to any one of claims 1 to 4 and / or the two-dimensional layered material prepared by the preparation method according to any one of claims 5 to 8; The positive electrode active material includes lithium cobalt oxide material and / or ternary material; The molecular formula of the lithium cobalt oxide material is LiCo m T 1-m O2, wherein T includes at least one of Mn, Al, Mg, Ti, Zr, Ca, Fe, and W, and 0.9≤m≤1.0; The molecular formula of the ternary material is LiNi x Co y N 1-x-y O2, wherein N includes at least one of Mn, Al, Mg, Ti, Zr, W, and B, 0.4≤x≤1.0, 0≤y≤0.4, and x+y≤1.0; The mass percentage of each component in the positive electrode active material layer is: Positive electrode active material 90%~99% Conductive agent 0.1%~9.8% Second binder 0.1%~9.8% Two-dimensional layered materials 0.1%~5%.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode sheet according to claim 9.
Citation Information
Patent Citations
High-nickel ternary positive electrode material containing active oxygen removing agent and preparation method thereof
CN110071278A
Lithium ion battery
CN211088320U