High strength cement mortar
By using slag powder and borax-sodium silicate composite activator in cement mortar, the problem of anionic polyacrylamide residue affecting the strength of cement mortar is solved, the effect of improving the strength and fluidity of mortar is achieved, and the porosity and dry shrinkage are reduced. Phenomenon.
Patent Information
- Application Number
- CN202410723175.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-05
AI Technical Summary
The anionic polyacrylamide remaining in manufactured sand will reduce the strength of cement mortar, leading to increased porosity and reduced fluidity, affecting the performance of building materials.
By adding slag powder and borax-sodium silicate composite activator to cement mortar, the early hydration rate of slag powder is suppressed, the water retention of anionic polyacrylamide is reduced, and borate ions form a complex with Ca2+ to reduce pores rate and improve the later strength of mortar.
It effectively improves the strength and fluidity of cement mortar, reduces porosity, reduces dry shrinkage, improves the overall performance of building materials, and reduces the difficulty of anionic polyacrylamide impurity removal in machine-made sand production.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the field of cement mortar, and in particular to a high-strength cement mortar. Background Art
[0002] Artificial sand refers to sand processed by sand making machines and other ancillary equipment. It is a substitute for natural river sand. Its finished product is more regular and can be processed into sand of different rules and sizes according to different process requirements, which can better meet daily needs. In the sand washing step of artificial sand production, flocculant polyacrylamide (PAM) is introduced, among which anionic polyacrylamide (APAM) has the best effect as a flocculant, resulting in anionic polyacrylamide (APAM) residue in the produced artificial sand.
[0003] Anionic polyacrylamide (APAM) is a water-soluble polymer rich in hydrophilic carboxyl groups. It is very easy to adhere to the surface of cement particles during the cement mixing process, thereby enhancing the water retention of the mortar and reducing its fluidity. A small amount of anionic polyacrylamide (APAM) can significantly affect the performance of the mixture after hardening, causing the porosity to increase and the strength of the mortar to decrease. Summary of the invention
[0004] In order to reduce the influence of anionic polyacrylamide residue in machine-made sand on the strength of cement mortar, the present application provides a high-strength cement mortar.
[0005] The present application provides a high-strength cement mortar, which adopts the following technical solution:
[0006] High-strength cement mortar comprises the following components in parts by weight:
[0007] 95-105 parts of cement;
[0008] 60-70 parts of sand, containing 0.001-0.040% by mass of anionic polyacrylamide;
[0009] Admixture 0.5-0.8 parts;
[0010] 38-42 parts of slag powder;
[0011] 18-22 parts of borax-sodium silicate composite activator;
[0012] 38-42 parts of water.
[0013] By adopting the above technical solution, slag powder, as an industrial solid waste, has a large annual output. The addition of slag powder in mortar can better improve the strength of mortar and is a high-quality admixture in the construction industry. Slag powder is usually used with alkaline activators, but alkaline activators increase the hydration rate of slag powder and cement, resulting in greater shrinkage and easy cracking. Cracks accelerate the erosion of harmful media such as CO2 and acid-base ions. By using borax-sodium silicate composite activator, in the early stage of hydration, borate ions react with Ca 2+ Calcium borate complex is formed and attached to the surface of unreacted slag, thereby slowing down the condensation rate. The complex on the slag surface has semi-permeable membrane properties. As the hydration reaction proceeds, the complex is continuously penetrated and destroyed, making the mortar hydration reaction tend to be normal, thus inhibiting the early hydration rate of the mortar, reducing shrinkage, and reducing the generation of pores. In addition, the semi-permeable membrane properties of the complex on the slag surface will not affect the later hydration strength, so that the mortar is fully hydrated and the later mortar strength is improved.
[0014] The residual anionic polyacrylamide will reduce the water seepage rate of cement mortar, has water retention, and is conducive to early hydration. However, as hydration proceeds, more pores are generated due to water loss, and the hydration products produced cannot fill the pores well, resulting in large porosity in the later stage and reduced strength of the mortar in the later stage. In addition, the carboxyl side chains generated by the hydrolysis of anionic polyacrylamide undergo ionic bonding with the cations of cement hydration products, which hinder the dispersion of cement particles. The gelling substances generated by complexation will also adhere to the surface of cement particles to increase the particle diameter in the liquid phase, resulting in uneven distribution of components and increased water demand for the entire system. After hydration, the pores generated by water loss in the later stage also increase, reducing the strength of the mortar.
[0015] After the slag powder is added, the anionic polyacrylamide hydrolyzes to produce carboxyl groups that preferentially attach to the surface of the slag powder, consuming polyacrylamide, thereby reducing its water retention. At the same time, the gelling substances generated by complexation attach to the surface of the slag, which, on the one hand, reduces the hydration rate of the slag powder and also improves the compatibility of the slag powder and cement base; on the other hand, due to the combination of anionic polyacrylamide with the slag powder, it is not easy to aggregate the cement into large particles, thereby reducing the water demand.
[0016] In this application, the complex produced by borax and anionic polyacrylamide is attached to the surface of slag powder, which inhibits the early hydration rate of slag powder on the one hand, and reduces the water retention caused by anionic polyacrylamide on the other hand, while also reducing the water demand, reducing the overall porosity and shrinkage, and improving the later mortar strength. The presence of anionic polyacrylamide in machine-made sand will not only not reduce the mortar strength, but will increase the mortar strength, and the mass percentage of anionic polyacrylamide in machine-made sand can reach 0.001-0.040%, greatly reducing the difficulty of removing impurities from anionic polyacrylamide during machine-made sand production.
[0017] Optionally, the mass percentage of anionic polyacrylamide is 0.020-0.026%.
[0018] By adopting the above technical solution, at this content, anionic polyacrylamide has a better effect on improving the strength of mortar.
[0019] Optionally, the mass percentage of anionic polyacrylamide is 0.023%.
[0020] Optionally, the borax-sodium silicate composite activator is prepared by the following method: solid sodium hydroxide is dissolved in water to obtain a solution, liquid sodium silicate is poured into the solution while stirring, and the modulus of the sodium silicate is adjusted to 1.2; then borax is added, stirred and mixed, and allowed to stand for 8-16 hours, and the mass ratio of the added borax to the liquid sodium silicate is 1:(4.2-4.5), and the borax-sodium silicate composite activator does not contain water added during the preparation process.
[0021] By adopting the above technical scheme, a borax-sodium silicate composite activator is prepared.
[0022] Optionally, the admixture is a dry powder defoamer.
[0023] By adopting the above technical solution, foam is eliminated, the porosity of the mortar is reduced, and the strength of the mortar is improved.
[0024] Optionally, the preparation method is as follows: divide water into three parts, the first part of water is used for the preparation of borax-sodium silicate composite activator, the slag powder and sand are stirred and mixed evenly, the second part of water is added and stirred and mixed evenly at 50-60°C, and then the borax-sodium silicate composite activator is added and stirred evenly, and finally the admixture, cement and the third part of water are added and stirred and mixed evenly, and the preparation is completed.
[0025] By adopting the above technical scheme, a borax-sodium silicate composite activator is first prepared, and the activator is left to stand for a period of time for use. Then, slag powder and sand are stirred and mixed, and then water is added, so that the anionic polyacrylamide in the sand first adheres to the surface of the slag powder, inhibits the early hydration of the slag powder and reduces the water retention of the anionic polyacrylamide. Under the condition of 50-60°C, the hydrolysis of the anionic polyacrylamide is facilitated; then, the borax-sodium silicate composite activator is added to better coat the surface of the slag powder, further reducing the early hydration rate of the slag powder, and finally, cement and water are added to prepare the mortar.
[0026] In summary, the present application includes at least one of the following beneficial technical effects:
[0027] The complex produced by borax and anionic polyacrylamide is attached to the surface of slag powder, which inhibits the early hydration rate of slag powder on the one hand, and reduces the water retention caused by anionic polyacrylamide on the other hand, while also reducing water demand, reducing overall porosity and shrinkage, and improving the strength of the mortar in the later stage. The presence of anionic polyacrylamide in machine-made sand will not only not reduce the strength of the mortar, but will increase it. The mass percentage of anionic polyacrylamide in machine-made sand can reach 0.001-0.040%, which greatly reduces the difficulty of removing impurities from anionic polyacrylamide during the production of machine-made sand.
[0028] The mass percentage of anionic polyacrylamide is set to 0.020-0.026% to make the mortar have better strength;
[0029] During preparation, sand and slag powder are preferably mixed at 50-60°C and then borax-sodium silicate composite activator, cement and defoamer are added to facilitate the hydrolysis of anionic polyacrylamide and its attachment to the slag powder, thereby improving the strength of the mortar. DETAILED DESCRIPTION
[0030] The present application is further described in detail below with reference to the embodiments.
[0031] Raw materials: Cement is Albo brand 42.5 grade silicate cement; slag powder is S95 grade slag powder, Erping brand, purchased from Erping Mineral Products Processing Plant in Lingshou County; river sand, passed through a 10-mesh sieve; anionic polyacrylamide, molecular weight 1000w; defoamer is a dry powder defoamer, Qingshuichi brand, pH 7; borax molecular formula: Na2B407, white particles; liquid sodium silicate, Jinyu brand, purchased from Jinan Jinyu Chemical Co., Ltd., with an initial modulus of 3.23 and a Baume degree of 41.3. Example Example 1
[0032] High-strength cement mortar comprises the following components in parts by weight:
[0033] 95 parts of cement;
[0034] 60 parts of sand, containing 0.001% by mass of anionic polyacrylamide;
[0035] 0.5 parts of defoaming agent;
[0036] 38 parts of slag powder;
[0037] 18 parts of borax-sodium silicate composite activator;
[0038] 38 parts water.
[0039] The sand containing anionic polyacrylamide is prepared by the following method: anionic polyacrylamide is weighed, added into water, stirred and dissolved, and then placed in a water bath at 60 degrees Celsius for 12 hours, then added into river sand, stirred and mixed evenly, to obtain sand containing 0.001% by mass of anionic polyacrylamide.
[0040] The borax-sodium silicate composite activator is prepared by the following method: solid sodium hydroxide is dissolved in water to obtain a solution, liquid sodium silicate is poured into the solution while stirring, and the modulus of the sodium silicate is adjusted to 1.2; then borax is added, stirred and mixed, and allowed to stand for 8 hours, and the mass ratio of the added borax to the liquid sodium silicate is 1:4.2. The borax-sodium silicate composite activator does not contain water added during the preparation process.
[0041] The preparation method of high-strength cement mortar is as follows: divide water into three parts according to the required mass, the first part of water is used for the preparation of borax-sodium silicate composite activator, the slag powder and sand are stirred and mixed evenly, the second part of water is added and stirred and mixed evenly at 50°C, and then the borax-sodium silicate composite activator is added and stirred evenly, and finally the admixture, cement and the third part of water are added and stirred and mixed evenly, and the preparation is completed. Example 2
[0042] High-strength cement mortar comprises the following components in parts by weight:
[0043] 100 parts of cement;
[0044] 65 parts of sand, containing 0.020% by mass of anionic polyacrylamide;
[0045] 0.65 parts of defoaming agent;
[0046] 40 parts of slag powder;
[0047] 20 parts of borax-sodium silicate composite activator;
[0048] 40 parts of water.
[0049] Sand containing anionic polyacrylamide is prepared by the following method: weigh anionic polyacrylamide, add it into water, stir and dissolve it, then stand it in a 60 degrees Celsius water bath for 12 hours, then add it into river sand, stir and mix evenly, and obtain sand containing 0.020% by mass of anionic polyacrylamide.
[0050] The borax-sodium silicate composite activator is prepared by the following method: solid sodium hydroxide is dissolved in water to obtain a solution, liquid sodium silicate is poured into the solution while stirring, and the modulus of the sodium silicate is adjusted to 1.2; then borax is added, stirred and mixed, and allowed to stand for 12 hours, and the mass ratio of the added borax to the liquid sodium silicate is 1:4.35. The borax-sodium silicate composite activator does not contain water added during the preparation process.
[0051] The preparation method of high-strength cement mortar is as follows: divide water into three parts according to the required mass, the first part of water is used for the preparation of borax-sodium silicate composite activator, the slag powder and sand are stirred and mixed evenly, the second part of water is added and stirred and mixed evenly at 55°C, and then the borax-sodium silicate composite activator is added and stirred evenly, and finally the admixture, cement and the third part of water are added and stirred and mixed evenly, and the preparation is completed. Example 3
[0052] High-strength cement mortar comprises the following components in parts by weight:
[0053] 105 parts of cement;
[0054] 70 parts of sand, containing 0.040% by mass of anionic polyacrylamide;
[0055] 0.8 parts of defoaming agent;
[0056] 42 parts of slag powder;
[0057] 22 parts of borax-sodium silicate composite activator;
[0058] 42 parts of water.
[0059] The sand containing anionic polyacrylamide is prepared by the following method: anionic polyacrylamide is weighed, added into water, stirred and dissolved, and then placed in a water bath at 60 degrees Celsius for 12 hours, then added into river sand, stirred and mixed evenly, to obtain sand containing 0.040% by mass of anionic polyacrylamide.
[0060] The borax-sodium silicate composite activator is prepared by the following method: solid sodium hydroxide is dissolved in water to obtain a solution, liquid sodium silicate is poured into the solution while stirring, and the modulus of the sodium silicate is adjusted to 1.2; then borax is added, stirred and mixed, and allowed to stand for 16 hours, and the mass ratio of the added borax to the liquid sodium silicate is 1:4.5. The borax-sodium silicate composite activator does not contain water added during the preparation process.
[0061] The preparation method of high-strength cement mortar is as follows: divide water into three parts according to the required mass, the first part of water is used for the preparation of borax-sodium silicate composite activator, the slag powder and sand are stirred and mixed evenly, the second part of water is added and stirred and mixed evenly at 60°C, and then the borax-sodium silicate composite activator is added and stirred evenly, and finally the admixture, cement and the third part of water are added and stirred and mixed evenly, and the preparation is completed. Example 4
[0062] The difference from Example 3 is that the mass percentage of anionic polyacrylamide in the sand is 0.023%. Example 5
[0063] The difference from Example 3 is that the mass percentage of anionic polyacrylamide in the sand is 0.026%.
[0064] Comparative Example
[0065] Comparative Example 1
[0066] The difference from Example 4 is that an equal amount of river sand not containing anionic polyacrylamide replaces sand.
[0067] Comparative Example 2
[0068] The difference from Example 4 is that an equal amount of river sand replaces the slag powder.
[0069] Comparative Example 3
[0070] The difference from Comparative Example 2 is that an equal amount of river sand not containing anionic polyacrylamide replaces sand.
[0071] Test piece production
[0072] The mortars prepared in the examples and comparative examples were placed in a test mold, demolded after curing for 24 hours, moved into a standard curing room and cured to the required age, and then taken out for testing.
[0073] Performance testing
[0074] Cement mortar fluidity test: Refer to "Cement mortar fluidity test method" (GB / T2419-2005) to test the mortar fluidity. The test results are recorded in Table 1.
[0075] Flexural strength and compressive strength test: refer to "Cement mortar strength test method" (GB / T17671-1999) for test, test the flexural strength and compressive strength of the specimens at 7d and 28d of curing respectively. The test results are recorded in Table 1. The flexural loading rate is 50N / s and the compressive loading rate is 2.4kN / s.
[0076] Apparent porosity test: The apparent porosity (P) of the pure slurry test block is measured using a 50mm×50mm×50mm specimen with a curing time of 28 days. The test is performed in accordance with the ASTM-C20 standard. First, the standard 28-day curing test block is placed in a vacuum water retaining machine for 24 hours, and the saturated weight W is measured after being taken out. Then the test block is placed in a hanging basket to measure the hanging weight S, and finally the test block is placed in an oven at 110°C for 24 hours and then the dry weight D is measured. The apparent porosity is calculated as follows:
[0077] Apparent porosity of pure slurry specimen (P) = [(saturated weight W-dry weight D) / (saturated weight W-hanging weight S)] × 100%
[0078] The test results are recorded in Table 1.
[0079] Table 1 Mortar test results
[0080]
[0081] Referring to the literature “Experimental study on shrinkage and microscopic properties of borax-sodium silicate alkali-activated slag mortar” Chen Haiming, Qin Ziguang, Chen Jie, Zhang Yadong, and Wu Peng, it has been pointed out that the addition of borax-sodium silicate helps to reduce the porosity of slag powder-mortar, and experimental analysis was carried out on this basis.
[0082] Analysis of test results:
[0083] 1. Fluidity
[0084] Combining Example 4 with Comparative Example 1 and Table 1, it can be seen that the addition of anionic polyacrylamide will greatly reduce the fluidity of the mortar. Compared with Comparative Example 1, the fluidity in Example 4 is reduced by 19 mm. It can be seen from Example 4 and Comparative Example 2 that the addition of slag powder improves the fluidity of the mortar because the water demand of slag powder is small. Compared with Comparative Example 2, the fluidity in Example 4 is improved by 12 mm.
[0085] It can be seen from the experimental data of Example 4 and Comparative Examples 1-2 that the ability of adding anionic polyacrylamide alone to reduce the fluidity of the mortar is significantly stronger than the ability of adding slag powder alone to improve the fluidity of the mortar; however, in combination with Comparative Example 3, it can be seen that when neither slag powder nor anionic polyacrylamide is added, the fluidity in Example 4 is increased by 5 mm compared with Comparative Example 3, and the fluidity of the mortar is improved, that is, the slag powder can inhibit the anionic polyacrylamide from reducing the fluidity of the mortar. The reason may be that the anionic polyacrylamide is combined with the surface of the slag powder, reducing the water retention performance of the anionic polyacrylamide.
[0086] 2. Strength and Porosity Analysis
[0087] Combining Examples 1-5 and Table 1, it can be seen that when the content of anionic polyacrylamide added to the sand is 0.23%, the mortar strength is the best. If an excessive amount is added, the anionic polyacrylamide will increase the mortar porosity and reduce the mortar strength; when the amount added is insufficient, the anionic polyacrylamide is difficult to be well coated on the surface of the slag powder, resulting in an increase in the hydration rate of the slag powder, an increase in the number and size of the pores, and an impact on the mortar strength.
[0088] Combining Example 4 and Comparative Examples 1-3, it can be seen that the addition of anionic polyacrylamide alone can significantly reduce the mortar strength and increase the mortar porosity. After adding slag powder alone, although the strength is increased, the porosity is large, which affects the mortar strength. By adding anionic polyacrylamide and slag powder together, the two work synergistically, and the porosity is reduced and the strength is increased compared to the addition of slag powder alone.
[0089] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. High-strength cement mortar, characterized in that: Contains the following components in parts by weight: 95-105 parts of cement; 60-70 parts of sand, containing 0.020-0.026% by mass of anionic polyacrylamide; Admixture 0.5-0.8 parts; 38-42 parts of slag powder; 18-22 parts of borax-sodium silicate composite activator; the borax-sodium silicate composite activator is prepared by the following method: solid sodium hydroxide is dissolved in water to obtain a solution, liquid sodium silicate is poured into the solution while stirring, and the modulus of the sodium silicate is adjusted to 1.2; then borax is added, stirred and mixed, and allowed to stand for 8-16 hours, and the mass ratio of the amount of borax added to the liquid sodium silicate is 1:(4.2-4.5); 38-42 parts of water.
2. The high-strength cement mortar according to claim 1, characterized in that: The mass percentage of anionic polyacrylamide is 0.023%.
3. The high-strength cement mortar according to claim 1, characterized in that: The admixture is dry powder defoamer.
4. The high-strength cement mortar according to claim 1, characterized in that: The preparation method is as follows: divide water into three parts, the first part of water is used for the preparation of borax-sodium silicate composite activator, slag powder and sand are stirred and mixed evenly, the second part of water is added and stirred and mixed evenly at 50-60°C, then the borax-sodium silicate composite activator is added and stirred evenly, finally an admixture, cement and the third part of water are added and stirred and mixed evenly, and the preparation is completed.
Citation Information
Patent Citations
Wear-resistant cement mortar, wear-resistant floor and preparation method thereof
CN102910885A
Whisker reinforcement-based self-leveling cement mortar and application thereof
CN106830851A
Method for effectively alleviating alkali-activated concrete dry-shrinkage cracking
CN109574609A
Environment-friendly masonry mortar and preparation method thereof
CN111548099A
Method for resisting negative effect of flocculating agent in machine-made sand and application
CN114920509A