Refractory ceramic product and preparation method thereof
By modifying the composite functions of kaolin, nano-tantalum oxide intercalation, coupling agent, niobium carbide and hafnium carbide, combined with discharge plasma hot press sintering technology, the mechanical strength, thermal conductivity and oxidation resistance of refractory ceramic products are solved. Problem, high performance and low cost refractory ceramic products are achieved.
Patent Information
- Application Number
- CN202410441603.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-04-12
AI Technical Summary
The existing refractory ceramic products have low mechanical strength, low thermal conductivity, poor oxidation resistance, complex manufacturing process and high cost, which limit their application and service life in harsh environments.
By modifying kaolin, nano-tantalum oxide intercalation improves mechanical properties; adding coupling agents to enhance cross-linking density and oxidation resistance; using the composite function of niobium carbide and hafnium carbide, combined with in-situ decomposition into pore technology to improve density and resistance High temperature; adopts discharge plasma hot press sintering process to reduce costs.
It significantly improves the mechanical properties, thermal conductivity and oxidation resistance of refractory ceramic products, reduces manufacturing costs, realizes stability and reliability in high-temperature environments, and improves application performance and use value.
Smart Images

Figure CN118290169B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic products, and specifically refers to a refractory ceramic product and a preparation method thereof. Background Art
[0002] With the advancement of science and technology and the continuous updating of industrial production technology, the technical level of refractory ceramic products is also constantly improving. The research and development and application of new materials have enabled refractory ceramic products to have higher temperature tolerance and longer service life. Refractory ceramic products have a wide range of applications and can provide excellent performance in a variety of different environments. The development of refractory ceramic products has become a hot topic for future research.
[0003] However, the refractory ceramic products in the existing technology generally have the following problems: the refractory ceramic products currently used usually have low mechanical strength, are brittle and easily broken, which limits their application under harsh conditions such as impact, pressure and wear; the thermal conductivity of refractory ceramic products on the market is low, which makes it difficult for them to maintain stable performance at high temperatures; the performance of refractory ceramic products mainly focuses on the following problems: poor mechanical strength, low thermal conductivity, poor oxidation resistance, etc.; although some existing technologies for refractory ceramic products can be put into use in the market, the manufacturing process is relatively complicated and requires multiple steps and high-temperature sintering processes, which makes their manufacturing cost high, the molding rate low and the production cycle long. Summary of the invention
[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a refractory ceramic product and a preparation method thereof. In order to solve the problems of poor mechanical strength, low thermal conductivity, poor oxidation resistance, etc. of the existing refractory ceramic products, the present invention invents a refractory ceramic product, by modifying kaolin, so that nano tantalum oxide is intercalated into kaolin. The nano tantalum oxide itself has high strength and hardness. Inserting it into the interlayer of kaolin can significantly improve the mechanical properties of the composite material, so that it maintains good stability and reliability in a high temperature environment, and improves the electrical and thermal conductivity of the material; adding a coupling agent can form hydrogen bonds with the hydroxyl groups or water molecules on the surface of kaolin, increase the crosslinking inside the kaolin density, thereby improving strength. At the same time, a protective film is formed on the surface of kaolin to prevent further erosion of kaolin by external substances, thereby improving heat resistance; niobium carbide and hafnium carbide are mixed and in-situ decomposition pore-forming technology is used to prepare ceramic products with composite functions, thereby improving density, having higher hardness, high temperature resistance and oxidation resistance; adding a binder can bond the ceramic products together to make them have higher strength and durability; the preparation method of refractory ceramic products provided by the present invention, through discharge plasma hot pressing sintering, through the dual effects of pressure and temperature, the density is greatly improved, the application of refractory ceramic products is effectively improved, and the cost is reduced.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows: The present invention provides a refractory ceramic product, and the refractory ceramic product comprises the following components by weight:
[0006] Niobium carbide: 40-60 parts;
[0007] Hafnium carbide: 40-60 parts;
[0008] Modified kaolin: 30-50 parts;
[0009] Binder: 1-10 parts.
[0010] Furthermore, the refractory ceramic product comprises the following components by weight:
[0011] Niobium carbide: 45-55 parts;
[0012] Hafnium carbide: 45-55 parts;
[0013] Modified kaolin: 35-45 parts;
[0014] Binder: 4-8 parts.
[0015] Furthermore, the modified kaolin comprises the following components by weight:
[0016] Kaolin: 60-70 parts;
[0017] Tantalum oxide: 10-20 parts;
[0018] Coupling agent: 1-10 parts.
[0019] Furthermore, the coupling agent is a mixture of a silane coupling agent and a titanate coupling agent in a mass ratio of 1:1, the purity of the tantalum oxide is 99.99%, and the particle size is 200 mesh.
[0020] Furthermore, the purity of the niobium carbide is 98%, and the particle size is 200 meshes; the purity of the hafnium carbide is 99.5%, and the particle size is 400 meshes; and the binder is one of lignin sulfonates.
[0021] The present invention also provides a method for preparing a refractory ceramic product, comprising the following steps:
[0022] Step 1: preparing modified kaolin, firstly, mixing kaolin and tantalum oxide evenly, adding a coupling agent, and obtaining the modified kaolin;
[0023] Step 2: pretreating niobium carbide and hafnium carbide to obtain mixed powder;
[0024] Step 3: Evenly mix the products of step 1 and step 2, press them into a desired shape and dry them, and then fire them in an arc furnace at a firing temperature of 1800-1900° C. to obtain the refractory ceramic product.
[0025] Furthermore, the pretreatment is spark plasma sintering, and the process of spark plasma sintering includes:
[0026] The niobium carbide and hafnium carbide are uniformly mixed and put into a spark plasma hot pressing sintering furnace for sintering. The sintering temperature is 1800-1900°C, the sintering pressure is 7.9-8.7KN, the sintering time is 5-10min, and after sintering, the temperature is uniformly lowered to 1000-1100°C, and then naturally cooled to room temperature, and the pressure is reduced to 0.
[0027] The beneficial effects achieved by adopting the above-mentioned present invention are as follows:
[0028] (1) By modifying kaolin, nano-tantalum oxide is intercalated into kaolin. Nano-tantalum oxide itself has high strength and hardness. Inserting it into the interlayer of kaolin can significantly improve the mechanical properties of the composite material, enable it to maintain good stability and reliability in high temperature environments, and improve the electrical and thermal conductivity of the material;
[0029] (2) Adding coupling agent can form hydrogen bonds with hydroxyl groups or water molecules on the surface of kaolin, increase the cross-linking density inside kaolin, thereby improving the strength. At the same time, a protective film is formed on the surface of kaolin to prevent further erosion of kaolin by external substances, thereby improving heat resistance;
[0030] (3) By mixing niobium carbide and hafnium carbide and using in-situ decomposition pore-forming technology, ceramic products with composite functions can be prepared, which have improved density, higher hardness, high temperature resistance and oxidation resistance;
[0031] (4) The addition of a binder can bond ceramic products together to give them greater strength and durability;
[0032] (5) The preparation method of the refractory ceramic product provided by the present invention, through spark plasma hot pressing sintering, greatly improves the density through the dual effects of pressure and temperature, effectively improves the application of refractory ceramic products and reduces costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the following description of the embodiments in conjunction with the accompanying drawings, in which:
[0034] Figure 1 This is a scanning electron microscope image of the refractory ceramic product prepared in Example 1 of the present invention;
[0035] Figure 2 This is a scanning electron microscope image of the refractory ceramic product prepared in Example 2 of the present invention;
[0036] Figure 3 This is a scanning electron microscope image of the refractory ceramic product prepared in Example 3 of the present invention;
[0037] Figure 4 This is a scanning electron microscope image of the refractory ceramic product prepared in Example 4 of the present invention;
[0038] Figure 5 This is a scanning electron microscope image of the refractory ceramic product prepared in Example 5 of the present invention. DETAILED DESCRIPTION
[0039] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0040] In the examples of the present invention, if there is no special description of raw materials or processing techniques, it is indicated that they are all conventional commercially available raw materials or conventional processing techniques in the art. Example 1
[0041] The present invention provides a refractory ceramic product, which comprises the following components by weight:
[0042] Niobium carbide: 45 parts;
[0043] Hafnium carbide: 45 parts;
[0044] Modified kaolin: 35 parts;
[0045] Binder: 4 parts.
[0046] The modified kaolin comprises the following components by weight:
[0047] Kaolin: 60 parts;
[0048] Tantalum oxide: 10 parts;
[0049] Coupling agent: 1 part.
[0050] The coupling agent is a mixture of a silane coupling agent and a titanate coupling agent in a mass ratio of 1:1, the purity of tantalum oxide is 99.99%, and the particle size is 200 mesh.
[0051] Among them, the purity of niobium carbide is 98%, the particle size is 200 mesh, the purity of hafnium carbide is 99.5%, the particle size is 400 mesh, and the binder is one of the lignin sulfonates, such as sodium lignin sulfonate.
[0052] The present invention also provides a method for preparing a refractory ceramic product, comprising the following steps:
[0053] Step 1: preparing modified kaolin, firstly, mixing kaolin and tantalum oxide evenly, adding a coupling agent, and obtaining modified kaolin;
[0054] Step 2: pretreating niobium carbide and hafnium carbide to obtain mixed powder;
[0055] Step 3: Evenly mix the products of step 1 and step 2, then press into a desired shape and dry, and then fire in an arc furnace at a firing temperature of 1800° C. to obtain a refractory ceramic product.
[0056] Among them, the pretreatment is spark plasma sintering, and the process of spark plasma sintering includes:
[0057] The niobium carbide and hafnium carbide are evenly mixed and put into a spark plasma hot pressing sintering furnace for sintering. The sintering temperature is 1800°C, the sintering pressure is 7.9KN, and the sintering time is 5 minutes. After sintering, the temperature is uniformly lowered to 1000°C, and then naturally cooled to room temperature, and the pressure drops to 0. Example 2
[0058] The present invention provides a refractory ceramic product, which comprises the following components by weight:
[0059] Niobium carbide: 48 parts;
[0060] Hafnium carbide: 48 parts;
[0061] Modified kaolin: 38 parts;
[0062] Binder: 5 parts.
[0063] The modified kaolin comprises the following components by weight:
[0064] Kaolin: 62 parts;
[0065] Tantalum oxide: 13 parts;
[0066] Coupling agent: 3 parts.
[0067] The coupling agent is a mixture of a silane coupling agent and a titanate coupling agent in a mass ratio of 1:1, the purity of tantalum oxide is 99.99%, and the particle size is 200 mesh.
[0068] Among them, the purity of niobium carbide is 98%, the particle size is 200 mesh, the purity of hafnium carbide is 99.5%, the particle size is 400 mesh, and the binder is one of the lignin sulfonates, such as sodium lignin sulfonate.
[0069] The present invention also provides a method for preparing a refractory ceramic product, comprising the following steps:
[0070] Step 1: preparing modified kaolin, firstly, mixing kaolin and tantalum oxide evenly, adding a coupling agent, and obtaining modified kaolin;
[0071] Step 2: pretreating niobium carbide and hafnium carbide to obtain mixed powder;
[0072] Step 3: Evenly mix the products of step 1 and step 2, then press into a desired shape and dry, and then fire in an arc furnace at a firing temperature of 1830° C. to obtain a refractory ceramic product.
[0073] Among them, the pretreatment is spark plasma sintering, and the process of spark plasma sintering includes:
[0074] The niobium carbide and hafnium carbide are evenly mixed and put into a spark plasma hot pressing sintering furnace for sintering. The sintering temperature is 1850°C, the sintering pressure is 8.2KN, and the sintering time is 7 minutes. After sintering, the temperature is uniformly lowered to 1150°C, and then naturally cooled to room temperature, and the pressure drops to 0. Example 3
[0075] The present invention provides a refractory ceramic product, which comprises the following components by weight:
[0076] Niobium carbide: 50 parts;
[0077] Hafnium carbide: 50 parts;
[0078] Modified kaolin: 40 parts;
[0079] Binder: 6 parts.
[0080] The modified kaolin comprises the following components by weight:
[0081] Kaolin: 65 parts;
[0082] Tantalum oxide: 15 parts;
[0083] Coupling agent: 6 parts.
[0084] The coupling agent is a mixture of a silane coupling agent and a titanate coupling agent in a mass ratio of 1:1, the purity of tantalum oxide is 99.99%, and the particle size is 200 mesh.
[0085] Among them, the purity of niobium carbide is 98%, the particle size is 200 mesh, the purity of hafnium carbide is 99.5%, the particle size is 400 mesh, and the binder is one of the lignin sulfonates, such as sodium lignin sulfonate.
[0086] The present invention also provides a method for preparing a refractory ceramic product, comprising the following steps:
[0087] Step 1: preparing modified kaolin, firstly, mixing kaolin and tantalum oxide evenly, adding a coupling agent, and obtaining modified kaolin;
[0088] Step 2: pretreating niobium carbide and hafnium carbide to obtain mixed powder;
[0089] Step 3: Evenly mix the products of step 1 and step 2, then press them into a desired shape and dry them, and then fire them in an arc furnace at a firing temperature of 1900° C. to obtain a refractory ceramic product.
[0090] Among them, the pretreatment is spark plasma sintering, and the process of spark plasma sintering includes:
[0091] The niobium carbide and hafnium carbide are evenly mixed and put into a spark plasma hot pressing sintering furnace for sintering. The sintering temperature is 1900°C, the sintering pressure is 8.5KN, and the sintering time is 8 minutes. After sintering, the temperature is uniformly lowered to 1100°C, and then naturally cooled to room temperature, and the pressure drops to 0. Example 4
[0092] The present invention provides a refractory ceramic product, which comprises the following components by weight:
[0093] Niobium carbide: 52 parts;
[0094] Hafnium carbide: 52 parts;
[0095] Modified kaolin: 42 parts;
[0096] Binder: 7 parts.
[0097] The modified kaolin comprises the following components by weight:
[0098] Kaolin: 68 parts;
[0099] Tantalum oxide: 17 parts;
[0100] Coupling agent: 8 parts.
[0101] The coupling agent is a mixture of a silane coupling agent and a titanate coupling agent in a mass ratio of 1:1, the purity of tantalum oxide is 99.99%, and the particle size is 200 mesh.
[0102] Among them, the purity of niobium carbide is 98%, the particle size is 200 mesh, the purity of hafnium carbide is 99.5%, the particle size is 400 mesh, and the binder is one of the lignin sulfonates, such as sodium lignin sulfonate.
[0103] The present invention also provides a method for preparing a refractory ceramic product, comprising the following steps:
[0104] Step 1: preparing modified kaolin, firstly, mixing kaolin and tantalum oxide evenly, adding a coupling agent, and obtaining modified kaolin;
[0105] Step 2: pretreating niobium carbide and hafnium carbide to obtain mixed powder;
[0106] Step 3: Evenly mix the products of step 1 and step 2, then press them into a desired shape and dry them, and then fire them in an arc furnace at a firing temperature of 1900° C. to obtain a refractory ceramic product.
[0107] Among them, the pretreatment is spark plasma sintering, and the process of spark plasma sintering includes:
[0108] The niobium carbide and hafnium carbide are evenly mixed and put into a spark plasma hot pressing sintering furnace for sintering. The sintering temperature is 1900°C, the sintering pressure is 8.7KN, and the sintering time is 10 minutes. After sintering, the temperature is uniformly lowered to 1100°C, and then naturally cooled to room temperature, and the pressure drops to 0. Example 5
[0109] The present invention provides a refractory ceramic product, which comprises the following components by weight:
[0110] Niobium carbide: 55 parts;
[0111] Hafnium carbide: 55 parts;
[0112] Modified kaolin: 45 parts;
[0113] Binder: 8 parts.
[0114] The modified kaolin comprises the following components by weight:
[0115] Kaolin: 70 parts;
[0116] Tantalum oxide: 20 parts;
[0117] Coupling agent: 10 parts.
[0118] The coupling agent is a mixture of a silane coupling agent and a titanate coupling agent in a mass ratio of 1:1, the purity of tantalum oxide is 99.99%, and the particle size is 200 mesh.
[0119] Among them, the purity of niobium carbide is 98%, the particle size is 200 mesh, the purity of hafnium carbide is 99.5%, the particle size is 400 mesh, and the binder is one of the lignin sulfonates, such as sodium lignin sulfonate.
[0120] The present invention also provides a method for preparing a refractory ceramic product, comprising the following steps:
[0121] Step 1: preparing modified kaolin, firstly, mixing kaolin and tantalum oxide evenly, adding a coupling agent, and obtaining modified kaolin;
[0122] Step 2: pretreating niobium carbide and hafnium carbide to obtain mixed powder;
[0123] Step 3: Evenly mix the products of step 1 and step 2, then press them into a desired shape and dry them, and then fire them in an arc furnace at a firing temperature of 1900° C. to obtain a refractory ceramic product.
[0124] Among them, the pretreatment is spark plasma sintering, and the process of spark plasma sintering includes:
[0125] The niobium carbide and hafnium carbide are evenly mixed and put into a spark plasma hot pressing sintering furnace for sintering. The sintering temperature is 1900°C, the sintering pressure is 8.7KN, and the sintering time is 10 minutes. After sintering, the temperature is uniformly lowered to 1100°C, and then naturally cooled to room temperature, and the pressure drops to 0.
[0126] Comparative Example 1
[0127] This comparative example provides a refractory ceramic product and a preparation method thereof, which differs from Example 1 only in that tantalum oxide and coupling agent are not included in the components, and the reduced amounts of tantalum oxide and coupling agent are distributed to kaolin, and the remaining components and component contents are the same as those in Example 1.
[0128] Comparative Example 2
[0129] This comparative example provides a refractory ceramic product and a preparation method thereof, which differs from Example 1 only in that the components do not contain hafnium carbide and niobium carbide, and the reduced amount of hafnium carbide and niobium carbide is distributed to kaolin, and the remaining components and component contents are the same as those in Example 1.
[0130] Comparative Example 3
[0131] This comparative example provides a refractory ceramic product and a preparation method thereof, which differs from Example 1 only in that tantalum oxide, coupling agent, hafnium carbide and niobium carbide are not included in the components, and the reduced amounts of tantalum oxide, coupling agent, hafnium carbide and niobium carbide are distributed to kaolin, and the remaining components and component contents are the same as those in Example 1.
[0132] The refractory ceramic products prepared in Examples 1-5 and Comparative Examples 1-3 were respectively subjected to fracture toughness and bending strength tests, and the test methods are as follows:
[0133] The mechanical properties test bars are processed through cutting, grinding, polishing and other processes. The fracture toughness test bar size is 4mm×6mm×30mm, the span is 24mm, and the cut height is about 2.5mm; the bending strength test bar size is 3mm×4mm×36mm, and the span is 30mm. A three-point bending test was carried out on a fixed displacement rate pressure tester to determine the fracture toughness value and bending strength respectively. The thermal conductivity of the sample was tested, and the thermal conductivity was obtained by the ST449 test, and the argon purge was 180ml / min, as shown in Table 1:
[0134] Table 1 Performance of a refractory ceramic product
[0135]
[0136] like Figure 1 , Figure 2 , Figure 3 , Figure 4 , Figure 5 As shown in Table 1, the fracture toughness, flexural strength, thermal conductivity, thermal stability limit temperature and density of the refractory ceramic products in the embodiments of the present invention are significantly higher than those in the comparative examples, indicating that the refractory ceramic products of the present invention have excellent properties such as high fracture toughness, flexural strength, thermal conductivity, thermal stability limit temperature and density, and can be produced on a large scale at low cost.
[0137] By adopting the preparation method of the refractory ceramic product provided by the present invention, the fracture toughness, bending strength, thermal conductivity, thermal stability limit temperature and density of Example 3 are optimal, and the fracture toughness reaches 6.6MPa*m 1 / 2 , bending strength reaches 456MPa, thermal conductivity reaches 40W / m*k, thermal stability limit temperature reaches 794K, and density reaches 99%. It can be seen that the introduced materials need to be within a certain amount, and adding too much or too little will affect the performance; while the performance of comparative examples 1, 2 and 3 is relatively poor, with no obvious difference. Therefore, considering the comprehensive performance of refractory ceramic products, the refractory ceramic products of the present invention can achieve strong fracture toughness and bending strength under high density conditions, improve excellent properties such as thermal conductivity and thermal stability limit temperature, and reduce costs at the same time. It has a high use value, thereby solving the problems of poor mechanical strength, low thermal conductivity, and poor oxidation resistance of existing refractory ceramic products.
[0138] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
[0139] The present invention and its implementation methods are described above, and such description is not restrictive, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the purpose of the invention, they can design structures and embodiments similar to the technical solution without creativity, which should all fall within the protection scope of the present invention.
Claims
1. A refractory ceramic product, characterized in that: The refractory ceramic product is composed of the following components by weight: 40-60 parts of niobium carbide, 40-60 parts of hafnium carbide, 30-50 parts of modified kaolin and 1-10 parts of a binder; The modified kaolin is composed of the following components by weight: 60-70 parts of kaolin, 10-20 parts of tantalum oxide and 1-10 parts of coupling agent; Wherein, the coupling agent is a mixture of a silane coupling agent and a titanate coupling agent in a mass ratio of 1:
1.
2. A refractory ceramic product according to claim 1, characterized in that: The refractory ceramic product consists of the following components by weight: 45-55 parts of niobium carbide, 45-55 parts of hafnium carbide, 35-45 parts of modified kaolin and 4-8 parts of a binder.
3. A refractory ceramic product according to claim 1, characterized in that: The purity of the tantalum oxide is 99.99% and the particle size is 200 mesh.
4. A refractory ceramic product according to claim 1, characterized in that: The purity of the niobium carbide is 98%, and the particle size is 200 meshes.
5. A refractory ceramic product according to claim 1, characterized in that: The purity of the hafnium carbide is 99.5%, and the particle size is 400 meshes.
6. A refractory ceramic product according to claim 1, characterized in that: The binder is a kind of lignin sulfonate.
7. The method for preparing a refractory ceramic product according to claim 1, characterized in that: The steps include: Step 1: preparing modified kaolin, firstly, mixing kaolin and tantalum oxide evenly, adding a coupling agent, and obtaining the modified kaolin; Step 2: pre-treating niobium carbide and hafnium carbide, wherein the pre-treatment is spark plasma sintering, and the spark plasma sintering process includes: mixing niobium carbide and hafnium carbide uniformly and putting them into a spark plasma hot pressing sintering furnace for sintering, the sintering temperature is 1800-1900° C., the sintering pressure is 7.9-8.7 KN, the sintering time is 5-10 min, and after sintering, the temperature is uniformly lowered to 1000-1100° C., and then naturally cooled to room temperature to obtain a mixed powder, and the pressure drop is 0; Step 3: Evenly mix the products of step 1 and step 2, press them into a desired shape and dry them, and then fire them in an arc furnace at a firing temperature of 1800-1900° C. to obtain the refractory ceramic product.
Citation Information
Patent Citations
Heat insulating composite and methods of manufacturing thereof
CN101193835A
Silicon carbide-molybdenum boride composite ceramic material and preparation method thereof
CN105777135A
Tantalum-containing refractory material for blast furnace ceramic cup and preparation method of tantalum-containing refractory material
CN113788689A
Composite conducting ceramic and its prepn
CN1453799A
Novel composite ceramics with improved toughness
WO1987004425A1