Silicone-polyurethane emulsion for hydrophobic finishing of polyester fabric and preparation method thereof

Through fluorine-free silicone-polyurethane emulsion, the cross-linked structure of branched and main chain silicones is combined with the surface of the fabric to solve the problem of insufficient water-repellent performance of fabrics in the existing technology and achieve a high-durability water-repellent effect. The combination with soft feel ensures safe and environmentally friendly use.

CN118290664BActive Publication Date: 2024-10-11YANGZHOU HONGCHENG NEW MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410453434.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-16
Publication Date
2024-10-11
Estimated Expiration
2044-04-16

AI Technical Summary

Technical Problem

It is difficult to improve the water-repellent performance and water-resistance of polyester fabrics without damaging the environment and human health with existing technology, especially because the use of fluorine-based water-repellent agents is risky, and it is difficult to improve the fabric with silicone water-repellent agents alone. Durable water repellent effect.

Method used

Using a fluorine-free silicone-polyurethane emulsion, a polyurethane emulsion of branched and main chain silicones is synthesized through a specific preparation method, and reacts with acrylic monomers through a cross-linked interpenetrating network structure to form a stable hydrophobic The group combines with the surface of the fabric to improve the water-repellent properties of the fabric.

Benefits of technology

It achieves a highly durable water-repellent effect on polyester fabrics, while giving the fabrics good softness and rich feel. The emulsion has high stability, is safe and environmentally friendly, and avoids the risk of using fluorine substances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004793429560000111
    Figure BDA0004793429560000111
  • Figure FDA0004999353110000011
    Figure FDA0004999353110000011
  • Figure FDA0004999353110000012
    Figure FDA0004999353110000012
Patent Text Reader

Abstract

This case involves a silicone-polyurethane emulsion for hydrophobic finishing of polyester fabrics and a preparation method thereof. First, three functional diol compounds with different structural formulas are obtained: A, B, and C; then polytetrahydrofuran and isophorone diisocyanate are used as raw materials to prepare polyurethane prepolymers, and then diol compounds A and B are used as chain extenders, and diol compound C is used as a chain extender to obtain polyurethane emulsions of branched silicone and polyurethane emulsions of main chain silicone; finally, it is polymerized with acrylic ester monomers. The silicone-polyurethane emulsion prepared by the present invention can be used as a water repellent in the hydrophobic finishing of polyester or nylon and its blended fabrics. The emulsion does not contain fluorine and solvent, and is safer to use; it can not only improve the durable water repellent effect of the fabric, but also has a high water resistance fastness; at the same time, it can also give polyester fabrics better softness and rich feel; the emulsion has high stability and good performance, and is a green and environmentally friendly water repellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of fabric treatment, in particular to an organosilicon-polyurethane emulsion for hydrophobic finishing of polyester fabric and a preparation method thereof. Background Art

[0002] With the progress of society and the improvement of living standards, people's requirements for textiles for clothing are getting higher and higher. After-finishing textiles with textile auxiliaries can effectively improve the performance of fabrics in various aspects. Polyester fiber has good elasticity and high strength, and is a type of textile material with high demand on the market, but polyester fiber also has the disadvantages of low moisture regain, poor hand feel, and easy static electricity, so textile auxiliaries are needed for finishing and modification. At present, the finishing of this type of fabric is mostly to improve the hydrophilicity and softness of the fabric. But for some special needs, it is hoped that the fabric has good water repellency. On the market, commonly used water repellents are mainly organosilicon compounds, reactive aliphatic compounds and organofluorine compounds. The fabric after finishing with reactive aliphatic compounds has a poor hand feel, so it is less used. CN111116920A discloses a branched multi-amino long-chain alkyl polysiloxane, a waterproof and soft organosilicon finishing agent, which needs to be used with an organic fluorine waterproofing agent to improve the softness and waterproofness of the fabric. However, fluorine-based water repellents are used on fabrics to cause certain harm to the environment and the human body, and their use should be minimized. However, it is difficult to improve the water resistance of the finished fabric by relying solely on the van der Waals force and hydrogen bonding force between the silicone water repellent and the fiber molecules. Summary of the invention

[0003] In view of the shortcomings of the prior art, the present invention designs a fluorine-free silicone emulsion, which can effectively improve the durable water-repellent effect of polyester fabrics by using the silicone emulsion for finishing, and also has high water resistance fastness.

[0004] To achieve the above object, the present invention provides the following technical solutions:

[0005] A method for preparing a silicone-polyurethane emulsion for hydrophobic finishing of polyester fabrics comprises the following steps:

[0006] 1) Firstly, a functional diol compound of the following structural formula is obtained;

[0007] Diol Compound A:

[0008] Diol Compound B:

[0009] Diol Compound C:

[0010] 2) Add a certain amount of polytetrahydrofuran to a stirred kettle, heat to 100°C and continue to evacuate for 60 minutes, cool to 50°C, add isophorone diisocyanate and a catalyst, introduce nitrogen protection, heat to 80°C, and react with stirring for 3 hours; cool to below 50°C, add an acetone solution mixed with diol compound A, heat to 70°C, and react for 2 hours; then add an acetone solution mixed with diol compound B, continue to react with stirring for 2-3 hours, cool to 50°C, add an oxime capping agent for capping, and obtain a polyurethane emulsion of branched silicone after self-emulsification;

[0011] 3) Add a certain amount of polytetrahydrofuran to a stirred tank, heat to 100°C and continue to evacuate for 60 minutes, cool to 50°C, add isophorone diisocyanate and a catalyst, introduce nitrogen protection, heat to 80°C, and stir to react for 3 hours; cool to below 50°C, add an acetone solution mixed with diol compound C, heat to 70°C, react for 2 hours, cool to 50°C, add an oxime capping agent for capping, and obtain a polyurethane emulsion of main chain silicone after self-emulsification;

[0012] 4) mixing the polyurethane emulsions obtained by the reaction of steps 2) and 3) in a certain proportion for later use;

[0013] 5) weighing octadecyl acrylate, butyl methacrylate and acrylic acid in a molar ratio of 2:1:0.5, mixing the acrylic ester monomers evenly, injecting the mixture into a polyether emulsifier aqueous solution and subjecting to ultrasound to obtain a miniemulsion;

[0014] 6) Add the mixed solution of step 4) into a reactor, add persulfate initiator thereto and stir evenly, then heat to 70-80° C., dropwise add the miniemulsion of step 5) into the reactor, keep the temperature for reaction for 3-5 hours after the dropwise addition is completed, and discharge the material after cooling.

[0015] Furthermore, the preparation process of the diol compound A is as follows:

[0016] Add equimolar amounts of glycidyl methacrylate and N-methyl monoethanolamine into a reaction flask, add ethanol solution, slowly raise the temperature to 70° C., stir to react overnight, cool and then perform reduced pressure distillation to obtain diol compound A.

[0017] Furthermore, the preparation process of the diol compound B is as follows:

[0018] S1, after dissolving octamethylcyclotetrasiloxane in a benzene solution, evacuate and seal with argon, take anhydrous and oxygen-free tetrahydrofuran, bring the above solution into a glove box, inject n-butyl lithium into a reaction bottle in the glove box, then first dropwise add the benzene solution mixed with octamethylcyclotetrasiloxane into the reaction bottle, after the dropwise addition is completed, add tetrahydrofuran to dilute, continue to stir and react overnight; take out the reaction bottle, add end-capping agent dimethylchlorosiloxane, continue to stir for 1h, and remove low-boiling substances by reduced pressure distillation to obtain single-end hydrogen siloxane;

[0019] S2. Add allyl isocyanate into the reaction flask and blow nitrogen for 30 minutes, then slowly dropwise add diethanolamine and stir to react for 2 to 3 hours to obtain an intermediate product containing a double bond;

[0020] S3. Mix the single-ended hydrogen siloxane and the toluene solution in a reaction bottle, add chloroplatinic acid-isopropanol solution, add a certain amount of the intermediate product containing double bonds in a constant pressure dropping funnel, blow nitrogen into the reaction bottle for 30 minutes, raise the temperature to 100°C, open the constant pressure dropping funnel, add the intermediate product containing double bonds drop by drop, stir the reaction for 5 to 6 hours, cool and distill under pressure to obtain diol compound B.

[0021] Furthermore, the polytetrahydrofuran in step 2) and step 3) is PTMG-1000; the catalyst is dibutyltin dilaurate; the oxime capping agent is selected from one of acetone oxime, butanone oxime, cyclohexanone oxime, and dimethylglyoxime; and the self-emulsification is to add a neutralizing agent and deionized water to emulsify to form an emulsion with a solid content of 30-40%.

[0022] Furthermore, in the step 2), the proportions of polytetrahydrofuran, isophorone diisocyanate, diol compound A, and diol compound B are: 20-25 parts, 23-27 parts, 5-8 parts, and 5-8 parts;

[0023] In the step 3), the proportions of polytetrahydrofuran, isophorone diisocyanate and diol compound C are: 20-25 parts, 23-27 parts and 8-10 parts.

[0024] Furthermore, in the step 4), the ratio of the polyurethane emulsion of the branched silicone to the polyurethane emulsion of the main-chain silicone is 1 to 3:1 based on the solid content.

[0025] Furthermore, in the step 5), the polyether emulsifier is alkylphenol polyoxyethylene ether or fatty alcohol polyoxyethylene ether, the amount of the polyether emulsifier is 2-3% by mass of the acrylic ester monomer mixture, and the solid content of the formed mini-emulsion is 30-40%.

[0026] Furthermore, in the step 6), the feed ratio of the mixed solution to the miniemulsion is 1:2 to 5 in terms of mass ratio based on the solid content therein.

[0027] Another object of the present invention is to provide a silicone-polyurethane emulsion for hydrophobic finishing of polyester fabrics prepared by the preparation method as described above.

[0028] Compared with the prior art, the present invention has the following beneficial effects: the organosilicon-polyurethane emulsion prepared by the present invention can be used as a water repellent in the hydrophobic finishing of polyester or nylon and their blended fabrics; the emulsion does not contain fluorine and solvent, and is safer to use; it can not only improve the durable water repellent effect of the fabric, but also has high water resistance fastness; at the same time, it can also give the polyester fabric better softness and rich hand feel; the emulsion has high stability and good performance, and is a green and environmentally friendly water repellent. DETAILED DESCRIPTION

[0029] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0031] Embodiment: A method for preparing a silicone-polyurethane emulsion for hydrophobic finishing of polyester fabrics comprises the following steps:

[0032] 1) Firstly, a functional diol compound of the following structural formula is obtained;

[0033] Diol Compound A: The preparation process is as follows:

[0034] Add equimolar amounts of glycidyl methacrylate and N-methyl monoethanolamine into a reaction flask, add ethanol solution, slowly raise the temperature to 70° C., stir to react overnight, cool and then perform reduced pressure distillation to obtain diol compound A.

[0035] Diol Compound B: Referring to the master's thesis "Synthesis and Performance Research of Polysiloxane Grafted on Block Modified Polyurethane Aqueous Dispersion", the product was prepared after deformation and improvement. The preparation process is as follows:

[0036] S2-1, dissolving octamethylcyclotetrasiloxane in a benzene solution, evacuating the solution, filling it with argon and sealing it, taking anhydrous and oxygen-free tetrahydrofuran, bringing the solution into a glove box, injecting n-butyl lithium into a reaction bottle in the glove box, and then dropping the benzene solution mixed with octamethylcyclotetrasiloxane into the reaction bottle drop by drop, adding tetrahydrofuran to dilute after the addition is complete, and continuing to stir the reaction overnight; taking out the reaction bottle, adding a capping agent dimethylchlorosiloxane, continuing to stir for 1 hour, and removing low-boiling substances by vacuum distillation to obtain single-end hydrogen siloxane;

[0037] S2-2, add allyl isocyanate into the reaction bottle and blow nitrogen for 30 minutes, slowly add diethanolamine dropwise and stir to react for 2 to 3 hours to obtain an intermediate product containing a double bond

[0038] S2-3, the single-end hydrogen siloxane and the toluene solution were mixed in a reaction bottle, a catalytic amount of chloroplatinic acid-isopropanol solution was added, a certain amount of the intermediate product containing double bonds was added to the constant pressure dropping funnel, nitrogen was introduced into the reaction bottle for 30 minutes, the temperature was raised to 100°C, the constant pressure dropping funnel was opened, the intermediate product containing double bonds was added dropwise, the reaction was stirred for 5 to 6 hours, and the diol compound B was obtained by pressure distillation after cooling. The molecular weight of the diol compound B finally obtained was 1800 g / mol.

[0039] Diol Compound C: Purchased from Anhui Mingyi Silicon Industry Co., Ltd., hydroxyl content is 8%, double bond content is 6%.

[0040] In this embodiment, the applicant selected three diol compounds composed of different functional groups. Diol compound A has a methacrylate structure, and the terminal double bond has a high free radical polymerization activity. It can undergo free radical polymerization with acrylate monomers, thereby increasing the active sites for the subsequent introduction of polyacrylate to form a cross-linked structure; diol compound B is a single-terminal diol compound formed by a single-terminal hydrogen polysiloxane, which is different from conventional double-terminal hydroxyl polysiloxane. The siloxane structure introduced by the reaction of diol compound B with a polyurethane prepolymer is suspended on the side chain of the polyurethane main chain rather than on the main chain, so that the siloxane structure contacts the fabric surface, and also facilitates the formation of chain entanglements in the subsequent graft polymerization reaction, thereby forming a structurally stable inter-conducting network structure.

[0041] Diol compound C is directly purchased and is a traditional double-terminal hydroxyl siloxane, and the side chain forms a carbon-carbon double bond. Diol compound C is selected to obtain a traditional polyurethane containing siloxane in the main chain. The introduction of a siloxane structure in the main chain structure of the polyurethane can effectively improve the softness of the finished fabric, but it does not have a durable water-repellent effect, and direct use cannot achieve the desired effect. However, the raw material is easy to obtain, the process for preparing polyurethane emulsion is simple, and the cost is relatively low, so it can be used as an auxiliary additive material, and the selected diol compound also has a polymerizable carbon-carbon double bond, which can also be used to increase the active site for the subsequent introduction of polyacrylate to form a cross-linked structure.

[0042] In the technical scheme of the present application, after forming a prepolymer with polytetrahydrofuran and isophorone isocyanate, diol compound A and diol compound B are added thereto to form a branched polyurethane emulsion containing silicone, and diol compound C is added to form a main chain polyurethane emulsion containing silicone, and both structures contain active double bonds. After mixing the two polyurethane emulsions, they are emulsified with acrylic monomers to form a cross-linked interpenetrating network structure, thereby making the prepared emulsion more stable. The polyurethane terminated by an oxime-type capping agent undergoes an unblocking reaction under high temperature conditions, and the -NCO group is released again, which has a strong activity and can react with the active groups on the fabric to improve the bonding strength of the polymer and the fabric. In addition, the long carbon chain alkyl segments are directional arranged on the surface of the fabric fiber, and a large number of hydrophobic groups also significantly improve the water repellency of the fabric, and the rich amide, ester, piperazine and other molecular segments in the emulsion form eutectics with the molecular segments of the fabric fibers, which also makes the finished fabric have higher water repellency and durability.

[0043] 2) Add 20 parts of polytetrahydrofuran to a stirred kettle, heat to 100°C and continue to evacuate for 60 minutes, cool to 50°C, add 25 parts of isophorone diisocyanate and 0.05 parts of dibutyltin dilaurate as a catalyst, introduce nitrogen protection, heat to 80°C, and react with stirring for 3 hours; cool to below 50°C, add acetone solution mixed with 5 parts of diol compound A, heat to 70°C, and react for 2 hours; then add acetone solution mixed with 6 parts of diol compound B, continue to react with stirring for 2-3 hours, cool to 50°C, add 3 parts of oxime blocking agent butanone oxime for blocking, cool to room temperature after the reaction is completed, add 2.5 parts of neutralizer for neutralization for 5 minutes, then slowly add deionized water under rapid stirring for self-emulsification to make the solid content at 30-40%, and obtain a polyurethane emulsion of branched silicone;

[0044] 3) Add 20 parts of polytetrahydrofuran to a stirred kettle, heat to 100° C. and continue to evacuate for 60 minutes, cool to 50° C., add 25 parts of isophorone diisocyanate and 0.05 parts of dibutyltin dilaurate as a catalyst, introduce nitrogen protection, heat to 80° C., stir and react for 3 hours; cool to below 50° C., add acetone solution mixed with 10 parts of diol compound C, heat to 70° C., react for 2 hours, cool to 50° C., add 3 parts of oxime-type blocking agent butanone oxime for blocking, cool to room temperature after the reaction is completed, add 2.5 parts of a neutralizing agent for neutralization for 5 minutes, then slowly add deionized water under rapid stirring for self-emulsification to make the solid content at 30-40%, and obtain a polyurethane emulsion of main chain silicone;

[0045] 4) adjusting the solid content of the polyurethane emulsions obtained in steps 2) and 3) to 35%, and mixing them in a mass ratio of 1 to 3:1 for later use;

[0046] 5) Weighing octadecyl acrylate, butyl methacrylate and acrylic acid in a molar ratio of 2:1:0.5, uniformly mixing the acrylate monomers, injecting the mixture into an aqueous solution of fatty alcohol polyoxyethylene ether or alkylphenol polyoxyethylene ether, and obtaining a miniemulsion by ultrasound; the amount of the polyether emulsifier is 2-3% of the mass of the acrylate monomer mixture, and the solid content of the formed miniemulsion is 30-40%.

[0047] 6) The mixed solution of step 4) is added to the reactor so that the mass ratio of the solid content of the mixed solution to the miniemulsion is 1:2-5, and a persulfate initiator is added thereto and stirred evenly, and the temperature is raised to 70-80° C. The miniemulsion of step 5) is added dropwise to the reactor. After the addition is completed, the reaction is kept warm for 3-5 hours, and the material is discharged after cooling.

[0048] Embodiment 1:

[0049] According to the above steps, a polyurethane emulsion of a branched silicone with a solid content of 35% and a polyurethane emulsion of a main-chain silicone are prepared respectively, and the mixture is mixed in a mass ratio of 1:1 for later use;

[0050] Weigh octadecyl acrylate, butyl methacrylate and acrylic acid in a molar ratio of 2:1:0.5, mix the acrylate monomers evenly, inject the mixture into a fatty alcohol polyoxyethylene ether or alkylphenol polyoxyethylene ether aqueous solution, and obtain a miniemulsion by ultrasound; the amount of the polyether emulsifier is 2-3% of the mass of the acrylate monomer mixture, and the solid content of the formed miniemulsion is 35%.

[0051] The mixed liquid is added into the reactor, and persulfate initiator is added thereto and stirred evenly, then the temperature is raised to 70-80°C, and the miniemulsion is added dropwise into the reactor so that the mass ratio of the mixed liquid to the miniemulsion is 1:2. After the addition is completed, the reaction is kept warm for 3-5 hours, and the material is discharged after the temperature is lowered.

[0052] Embodiment 2:

[0053] According to the above steps, a polyurethane emulsion of a branched silicone with a solid content of 35% and a polyurethane emulsion of a main-chain silicone were prepared respectively, and mixed in a mass ratio of 1:2 for later use.

[0054] Weigh octadecyl acrylate, butyl methacrylate and acrylic acid in a molar ratio of 2:1:0.5, mix the acrylate monomers evenly, inject the mixture into a fatty alcohol polyoxyethylene ether or alkylphenol polyoxyethylene ether aqueous solution, and obtain a miniemulsion by ultrasound; the amount of the polyether emulsifier is 2-3% of the mass of the acrylate monomer mixture, and the solid content of the formed miniemulsion is 35%.

[0055] The mixed liquid is added into the reactor, and persulfate initiator is added thereto and stirred evenly, then the temperature is raised to 70-80°C, and the miniemulsion is added dropwise into the reactor so that the mass ratio of the mixed liquid to the miniemulsion is 1:2. After the addition is completed, the reaction is kept warm for 3-5 hours, and the material is discharged after the temperature is lowered.

[0056] Embodiment 3:

[0057] According to the above steps, a polyurethane emulsion of a branched silicone with a solid content of 35% and a polyurethane emulsion of a main-chain silicone were prepared respectively, and mixed in a mass ratio of 1:3 for later use.

[0058] Weigh octadecyl acrylate, butyl methacrylate and acrylic acid in a molar ratio of 2:1:0.5, mix the acrylate monomers evenly, inject the mixture into a fatty alcohol polyoxyethylene ether or alkylphenol polyoxyethylene ether aqueous solution, and obtain a miniemulsion by ultrasound; the amount of the polyether emulsifier used accounts for 2.5% of the mass of the acrylate monomer mixture, and the solid content of the formed miniemulsion is 35%.

[0059] The mixed liquid is added into the reactor, and persulfate initiator is added thereto and stirred evenly, then the temperature is raised to 70-80°C, and the miniemulsion is added dropwise into the reactor so that the mass ratio of the mixed liquid to the miniemulsion is 1:2. After the addition is completed, the reaction is kept warm for 3-5 hours, and the material is discharged after the temperature is lowered.

[0060] Embodiment 4:

[0061] According to the above steps, a polyurethane emulsion of a branched silicone with a solid content of 35% and a polyurethane emulsion of a main-chain silicone were prepared respectively, and mixed in a mass ratio of 1:2 for later use.

[0062] Weigh octadecyl acrylate, butyl methacrylate and acrylic acid in a molar ratio of 2:1:0.5, mix the acrylate monomers evenly, inject the mixture into a fatty alcohol polyoxyethylene ether or alkylphenol polyoxyethylene ether aqueous solution, and obtain a miniemulsion by ultrasound; the amount of the polyether emulsifier used accounts for 2.5% of the mass of the acrylate monomer mixture, and the solid content of the formed miniemulsion is 35%.

[0063] The mixed liquid is added into the reactor, and persulfate initiator is added thereto and stirred evenly, then the temperature is raised to 70-80°C, and the miniemulsion is added dropwise into the reactor so that the mass ratio of the mixed liquid to the miniemulsion is 1:3.5. After the addition is completed, the reaction is kept warm for 3-5 hours, and the material is discharged after the temperature is lowered.

[0064] Embodiment 5:

[0065] According to the above steps, a polyurethane emulsion of a branched silicone with a solid content of 35% and a polyurethane emulsion of a main-chain silicone were prepared respectively, and mixed in a mass ratio of 1:2 for later use.

[0066] Weigh octadecyl acrylate, butyl methacrylate and acrylic acid in a molar ratio of 2:1:0.5, mix the acrylate monomers evenly, inject the mixture into a fatty alcohol polyoxyethylene ether or alkylphenol polyoxyethylene ether aqueous solution, and obtain a miniemulsion by ultrasound; the amount of the polyether emulsifier used accounts for 2.5% of the mass of the acrylate monomer mixture, and the solid content of the formed miniemulsion is 35%.

[0067] The mixed liquid is added into the reactor, and persulfate initiator is added thereto and stirred evenly, then the temperature is raised to 70-80°C, and the miniemulsion is added dropwise into the reactor so that the mass ratio of the mixed liquid to the miniemulsion is 1:5. After the addition is completed, the reaction is kept warm for 3-5 hours, and the material is discharged after the temperature is lowered.

[0068] Comparative Example 1:

[0069] Compared with Example 1, except that the polyurethane emulsion does not contain branched silicone, the rest is the same.

[0070] Comparative Example 2:

[0071] According to the above steps, a polyurethane emulsion of a branched silicone with a solid content of 35% and a polyurethane emulsion of a main-chain silicone are respectively prepared, and the emulsions are mixed in a mass ratio of 1:1.

[0072] Chemical properties and characterization of silicone-polyurethane emulsions:

[0073] 1. Emulsion particle size and contact angle

[0074] 2. Emulsion stability: Place the emulsion in a high-speed centrifuge and centrifuge it at 2000 r / min for 20 min to observe whether the emulsion has abnormal phenomena such as stratification. The above results are recorded in Table 1.

[0075] Table 1

[0076] Appearance stability Particle size / nm Contact angle / ° Example 1 Milky white with a bluish tint Stablize 120 142 Example 2 Milky white with a bluish tint Stablize 110 136 Example 3 cream More stable 150 131 Example 4 Milky white with a bluish tint Stablize 120 145 Example 5 Milky white with a bluish tint Stablize 130 147 Comparative Example 1 turbid Layering -- -- Comparative Example 2 translucent Unstable 90 110

[0077] It can be seen from Table 1 that the emulsion prepared in the present application has good stability, and the particle size of the emulsion is between 110-130. Among them, the particle size of Example 3 is larger, resulting in slightly worse stability than other examples. This may be because the main chain silicone polyurethane content in the mixed liquid is relatively high, and its polymerization activity with acrylate monomers is low, resulting in relatively weak performance of the final emulsion; it can also be seen from Comparative Example 1 that when there is no branched silicone polyurethane at all, the emulsion becomes turbid after adding acrylate monomers for reaction, and the stability is poor. When the main chain silicone polyurethane is directly mixed with the branched silicone polyurethane, its centrifugal stability is relatively poor and the contact angle is low, indicating poor water repellency.

[0078] In order to verify the effect of the above emulsion on fabric finishing, the following specific application examples were carried out.

[0079] Finishing process:

[0080] Fabric→impregnation (two impregnations and two paddings, the padding rate is 80%)→pre-baking (90°C, 60s)→baking (140-170°C, 60-180s).

[0081] Test the properties of the finished fabric:

[0082] 3. The feel of the fabric after finishing: the feel of the original fabric is rated as level 1, the highest level is 5, the lowest level is 1, and the average value is taken from a group of five.

[0083] 4. Waterproofness of fabric after finishing, spray method to assess waterproof grade

[0084] 5. Washability of fabric after finishing.

[0085] The above results are recorded in Table 2.

[0086] Table 2

[0087]

[0088] It can be seen from the above table that the organosilicon-polyurethane emulsion prepared in the present application can be used as a water repellent for fabrics, so that the finished fabrics have good water repellency, excellent water resistance and soft hand feel.

[0089] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.

Claims

1. A method for preparing a silicone-polyurethane emulsion for hydrophobic finishing of polyester fabrics, It is characterized in that The steps include: 1) Firstly, a functional diol compound of the following structural formula is obtained; Diol Compound A: Diol Compound B: Diol Compound C: 2) Add a certain amount of polytetrahydrofuran to a stirred kettle, heat to 100°C and continue to evacuate for 60 minutes, cool to 50°C, add isophorone diisocyanate and a catalyst, introduce nitrogen protection, heat to 80°C, and react with stirring for 3 hours; cool to below 50°C, add an acetone solution mixed with diol compound A, heat to 70°C, and react for 2 hours; then add an acetone solution mixed with diol compound B, continue to react with stirring for 2-3 hours, cool to 50°C, add an oxime capping agent for capping, and obtain a polyurethane emulsion of branched silicone after self-emulsification; 3) Add a certain amount of polytetrahydrofuran to a stirred tank, heat to 100°C and continue to evacuate for 60 minutes, cool to 50°C, add isophorone diisocyanate and a catalyst, introduce nitrogen protection, heat to 80°C, and stir to react for 3 hours; cool to below 50°C, add an acetone solution mixed with diol compound C, heat to 70°C, react for 2 hours, cool to 50°C, add an oxime capping agent for capping, and obtain a polyurethane emulsion of main chain silicone after self-emulsification; 4) mixing the polyurethane emulsions obtained by the reaction of steps 2) and 3) in a certain proportion for later use; 5) weighing octadecyl acrylate, butyl methacrylate and acrylic acid in a molar ratio of 2:1:0.5, mixing the acrylic ester monomers evenly, injecting the mixture into a polyether emulsifier aqueous solution and subjecting to ultrasound to obtain a miniemulsion; 6) adding the mixed solution of step 4) into a reaction kettle, adding a persulfate initiator thereto and stirring evenly, heating to 70-80° C., dropping the miniemulsion of step 5) into the reaction kettle, keeping the temperature for reaction for 3-5 hours after the dropwise addition is completed, and discharging the material after cooling; In the step 2), the proportions of polytetrahydrofuran, isophorone diisocyanate, diol compound A, and diol compound B are: 20-25 parts, 23-27 parts, 5-8 parts, and 5-8 parts; In the step 3), the proportions of polytetrahydrofuran, isophorone diisocyanate, and diol compound C are: 20-25 parts, 23-27 parts, and 8-10 parts; In the step 4), the ratio of the polyurethane emulsion of the branched silicone to the polyurethane emulsion of the main-chain silicone is 1 to 3:1 based on the solid content.

2. The method for preparing the organosilicon-polyurethane emulsion for hydrophobic finishing of polyester fabrics according to claim 1, It is characterized in that The preparation process of the diol compound A is as follows: Add equimolar amounts of glycidyl methacrylate and N-methyl monoethanolamine into a reaction flask, add ethanol solution, slowly raise the temperature to 70° C., stir to react overnight, cool and then perform reduced pressure distillation to obtain diol compound A.

3. The method for preparing the organosilicon-polyurethane emulsion for hydrophobic finishing of polyester fabrics according to claim 1, It is characterized in that The preparation process of the diol compound B is as follows: S1, after dissolving octamethylcyclotetrasiloxane in a benzene solution, evacuate and seal with argon, take anhydrous and oxygen-free tetrahydrofuran, bring the above solution into a glove box, inject n-butyl lithium into a reaction bottle in the glove box, then first dropwise add the benzene solution mixed with octamethylcyclotetrasiloxane into the reaction bottle, after the dropwise addition is completed, add tetrahydrofuran to dilute, continue to stir and react overnight; take out the reaction bottle, add end-capping agent dimethylchlorosiloxane, continue to stir for 1h, and remove low-boiling substances by reduced pressure distillation to obtain single-end hydrogen siloxane; S2. Add allyl isocyanate into the reaction flask and blow nitrogen for 30 minutes, then slowly dropwise add diethanolamine and stir to react for 2 to 3 hours to obtain an intermediate product containing a double bond; S3. Mix the single-ended hydrogen siloxane and the toluene solution in a reaction bottle, add chloroplatinic acid-isopropanol solution, add a certain amount of the intermediate product containing double bonds in a constant pressure dropping funnel, blow nitrogen into the reaction bottle for 30 minutes, raise the temperature to 100°C, open the constant pressure dropping funnel, add the intermediate product containing double bonds drop by drop, stir the reaction for 5 to 6 hours, cool and distill under pressure to obtain diol compound B.

4. The method for preparing the organosilicon-polyurethane emulsion for hydrophobic finishing of polyester fabrics according to claim 1, It is characterized in that The polytetrahydrofuran in step 2) and step 3) is PTMG-1000; the catalyst is dibutyltin dilaurate; the oxime capping agent is selected from one of acetone oxime, butanone oxime, cyclohexanone oxime and dimethylglyoxime; and the self-emulsification is to add a neutralizing agent and deionized water to emulsify to form an emulsion with a solid content of 30-40%.

5. The method for preparing the organosilicon-polyurethane emulsion for hydrophobic finishing of polyester fabrics according to claim 1, It is characterized in that In the step 5), the polyether emulsifier is alkylphenol polyoxyethylene ether or fatty alcohol polyoxyethylene ether, and the amount of the polyether emulsifier is 2-3% of the mass of the acrylic ester monomer mixture. The solid content of the formed mini-emulsion is 30-40%.

6. The method for preparing the organosilicon-polyurethane emulsion for hydrophobic finishing of polyester fabrics according to claim 1, It is characterized in that In the step 6), the feeding ratio of the mixed solution to the miniemulsion is 1:2-5 by mass based on the solid content.

7. An organosilicon-polyurethane emulsion for hydrophobic finishing of polyester fabrics prepared by the preparation method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Branched polyamino long-chain alkyl polysiloxane and waterproof soft organosilicon finishing agent, and preparation methods thereof

    CN111116920A

  • Polyurethane-organopolysiloxanes

    CN107820527A

  • Polyurethane-acrylate water repellent agent prepared from side chain double bonds

    CN111004361A

  • Branched chain type organic silicon modified polyurethane elastomer and preparation method thereof

    CN112979962A

  • Organic silicon treating agent, preparation method thereof and powder containing organic silicon treating agent

    CN115960359A