A coating composition with sunscreen and water repellent function
By combining silicone modified water-based polyurethane acrylate emulsion with silica-modified sol, combined with ultraviolet absorbers, a new coating composition was prepared, which solved the environmental pollution problem of fluorine-containing compounds and achieved excellent fabrics It has water repellent moisture permeability and UV resistance, while improving the color fastness of water washing resistance and meeting green chemical requirements.
Patent Information
- Application Number
- CN202410582605.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-11
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-05-11
AI Technical Summary
The existing coating compositions impart water repellent properties to fabrics by adding fluorine-containing compounds, which have adverse effects on the human body and the environment.
A new coating composition was prepared by blending silicone modified aqueous polyurethane acrylate emulsion with silica modified sol, combined with benzotriazole ultraviolet absorbers and other additives, and by isocyanate groups and γ- The reaction of aminopropyltriethoxysilane forms functionalized titanium dioxide, and finally uses tripropylene glycol diacrylate to obtain a coating with excellent water repellency and moisture permeability.
It achieves excellent water-repellent and moisture-permeable properties of the fabric, and improves UV resistance and water-washing color fastness, avoids environmental pollution of fluorine-containing finishing agents, and meets green chemical requirements.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coating compositions, and in particular to a novel coating composition with sunscreen and water repellent functions. Background Art
[0002] With the gradual improvement of material living standards, people's requirements for textiles are also getting higher and higher. Textiles have gradually changed from the traditional demand for warmth in winter and coolness in summer to the functional demand for hygiene, health and comfort. Textiles also need to have multiple functions such as water and oil repellency, antistatic, washable and wearable, antibacterial, flame retardant, etc. Functional fabrics have been widely used in household textiles, environmental and health textiles, decorative and industrial textiles, national defense construction and cutting-edge science. The development of functional fabrics involves not only the textile and dyeing industries, but also the chemical fiber and fine chemical industries. However, its basis is to develop materials with these functions. There are two main ways to develop them. One is to develop functional fibers and then make functional textiles from these fibers; the other is to functionally finish ordinary textiles to make them functional. In the textile printing and dyeing industry, the functionalization of textiles is generally achieved through functional finishing, that is, with the help of functional finishing agents. Water repellent finishing is to apply a layer of water-repellent film that cannot be soaked by water on the fabric, but without closing the pores of the fabric, so that the fabric has both water repellent and breathable properties. Anti-ultraviolet finishing allows the fabric to absorb or reflect ultraviolet rays, thereby protecting the skin.
[0003] Fluorine-containing finishing agents used for the "three-proof" finishing of textiles, such as waterproof, oil-proof and anti-fouling, are difficult to degrade and easily accumulate in the human body. In addition, the release of fluorine compounds during and after finishing is also detrimental to the environment. With the increase of human environmental awareness, these non-environmentally friendly functional finishing agents are facing severe challenges from environmental protection regulations. Therefore, it is a general trend to find safe and environmentally friendly finishing methods to give textiles functionality. Summary of the invention
[0004] The purpose of the present invention is to provide a new type of coating composition with sunscreen and water repellent function to solve the following technical problems:
[0005] Existing coating compositions impart water-repellent properties to fabrics by adding fluorine-containing compounds, which has adverse effects on the human body and the environment.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A novel coating composition with sunscreen and water repellent function, comprising the following raw materials in parts by weight: 50-80 parts of silicone-modified waterborne polyurethane acrylate emulsion, 10-25 parts of UV protection additive, 8 parts of additive, and 1-3 parts of thickener PTF;
[0008] The preparation method of the silicone-modified waterborne polyurethane acrylate emulsion comprises the following steps:
[0009] A1: In a nitrogen atmosphere, polyether diol (average molecular weight 1000), isophorone diisocyanate, and dibutyltin dilaurate are added to a reaction kettle, the temperature is controlled at 80-90°C, and the reaction is kept warm for 1-3 hours. Dimethylolpropionic acid and acetone are added, and the reaction is kept warm for 1-3 hours. The temperature is controlled at 60-70°C. Hydroxyethyl methacrylate is added, and the reaction is kept warm for 1-3 hours. The temperature is controlled at 65-75°C, and the reaction is kept warm for 1-3 hours. The temperature is controlled at 35-45°C, triethylamine is added, and the reaction is kept warm for 0.5-1 hour. Deionized water is added, and the reaction is kept warm for 1-3 hours. Acetone is removed by rotary evaporation to obtain an aqueous polyurethane acrylate emulsion;
[0010] A2: Blending an aqueous polyurethane acrylate emulsion and a silica-modified sol to obtain an organosilicon-modified aqueous polyurethane acrylate emulsion.
[0011] As a further embodiment of the present invention, the addition ratio of polyether diol, isophorone diisocyanate, dibutyltin dilaurate, dihydroxymethylpropionic acid, acetone, hydroxyethyl methacrylate, triethylamine and deionized water in A1 is 10 g: 5-8 g: 0.3-0.4 g: 1-2 g: 25-50 mL: 5-8 g: 1.1-1.5 g: 30-60 mL.
[0012] As a further solution of the present invention: the mass ratio of the aqueous polyurethane acrylate emulsion and the silica-modified sol in A2 is 20-30:20-50.
[0013] As a further embodiment of the present invention: the preparation method of the silica modified sol comprises the following steps:
[0014] S1: In a nitrogen atmosphere, nano titanium dioxide, 2,4-toluene diisocyanate and toluene are added into a reaction kettle and dispersed evenly, the temperature is controlled at 80-90°C, the mixture is stirred for 6-12 hours, washed with anhydrous ethanol and dried to obtain component 1;
[0015] S2: Add component 1, γ-aminopropyltriethoxysilane and ethyl acetate into a reaction kettle, control the temperature at 50-60°C, keep the temperature for reaction for 3-6 hours, add anhydrous ethanol to disperse evenly, keep the temperature for reaction for 1-3 hours, filter and dry to obtain component 2;
[0016] S3: Add anhydrous ethanol, component 2, and tetraethyl orthosilicate into a reaction kettle and disperse them evenly, dropwise add acetic acid solution, control the temperature at 25-35°C, and keep the reaction warm for 6-12 hours to obtain component 3;
[0017] S4: Add components three and tripropylene glycol diacrylate into a reaction kettle and disperse them evenly, and remove the solvent by distillation under reduced pressure to obtain a silica-modified sol.
[0018] As a further solution of the present invention: the addition ratio of nano titanium dioxide, 2,4-toluene diisocyanate and toluene in S1 is 10g: 10-15g: 100-300mL.
[0019] As a further solution of the present invention: the addition ratio of component 1, γ-aminopropyltriethoxysilane, ethyl acetate and anhydrous ethanol in S2 is 10g:15-20g:100-300mL:2-20mL.
[0020] As a further solution of the present invention: the acetic acid solution in S3 is 0.2-0.3 mol / L acetic acid solution, and the addition ratio of anhydrous ethanol, component two, tetraethyl orthosilicate, and acetic acid solution is 15-25 mL: 10 g: 4-12.5 g: 10-25 mL.
[0021] As a further solution of the present invention: the mass ratio of component three to tripropylene glycol diacrylate in S4 is 1:0.3-0.6.
[0022] As a further embodiment of the present invention: the anti-ultraviolet auxiliary agent is a benzotriazole ultraviolet absorber.
[0023] As a further solution of the present invention, the auxiliary agent includes 0.2-0.5 parts of dispersant, 0.5-1 parts of defoamer, 2-4 parts of moisturizer, 5-8 parts of water-based wax emulsion feel agent, 0.3-0.5 parts of pH regulator
[0024] As a further embodiment of the present invention: a method for preparing a coating composition comprises the following steps:
[0025] A1: Clean the dispersion tank, add the silicone-modified water-based polyurethane acrylate emulsion and UV protection additive into the tank and disperse them evenly to form a premix;
[0026] A2: Add additives to the premix while stirring and disperse evenly;
[0027] A3: Add thickener PTF and disperse evenly to obtain a coating composition.
[0028] The novel coating composition with sunscreen and water repellent function prepared by any one of the above methods is applied in fabric printing.
[0029] As a further solution of the present invention: the coating composition prepared in the present application is suitable for fabrics including windbreaker fabrics, pure cotton, spandex, and polyester fabrics.
[0030] As a further scheme of the present invention: a method for preparing a fabric with sunscreen and water repellent effect: using any of the above-mentioned novel coating compositions with sunscreen and water repellent function as printing paste; directly printing with 100% printing paste (recommended mesh: 800-1000 mesh), drying with hot air, and baking at a high temperature of 150-160°C for 2-3 minutes to obtain a fabric with sunscreen and water repellent effect.
[0031] Beneficial effects of the present invention:
[0032] (1) This application uses excess 2,4-toluene diisocyanate to modify the surface of titanium dioxide nanoparticles to synthesize functionalized titanium dioxide with -NCO groups on the surface, as component one; and uses the isocyanate group on component one to react with the amino group of γ-aminopropyltriethoxysilane to obtain nano titanium dioxide modified by a silane coupling agent, as component two; using component two and tetraethyl orthosilicate as precursors, synthesize titanium dioxide modified silica sol; finally, use tripropylene glycol diacrylate for secondary modification to obtain silica modified sol. This application uses polyether diol and isophorone diisocyanate to prepare polyurethane prepolymer under the catalysis of dibutyltin dilaurate, and adds acrylic monomer to prepare waterborne polyurethane acrylate emulsion; finally, the waterborne polyurethane acrylate emulsion and the silica modified sol are blended to obtain silicone modified waterborne polyurethane acrylate emulsion. The silicone-modified waterborne polyurethane acrylate emulsion prepared in the present application is used as a finishing agent and assisted by other functional additives to prepare a coating composition. The coating composition prepared in the present application is used to finish fabrics, giving the fabrics excellent water-repellent, moisture-permeable and UV-resistant properties, and high color fastness to washing.
[0033] The present application starts with titanium dioxide, and carries out organosilicon treatment through isocyanate and silane coupling agent, and introduces the special molecular composition and molecular structure of organosiloxane on the surface of titanium dioxide, which combines the characteristics of organic matter and the functions of inorganic matter, and has excellent water resistance and low surface tension; long-chain aliphatic hydrocarbon siloxane is used as a water repellent to replace fluorine-containing compounds to be grafted on the surface of titanium dioxide, and the hydrolyzed end of the silane coupling agent is modified to modify the silica hydrosol prepared based on tetraethyl orthosilicate, so that the coating composition can achieve a water repellent effect similar to that after finishing with a fluorine-containing finishing agent, so that the finishing process is economical, safe, good for the environment, and meets the requirements of green chemistry.
[0034] The present application utilizes silica-modified sol to modify polyurethane-acrylate, which is beneficial to reducing the surface energy of the material and improving the water resistance of the material. The silica is evenly dispersed in the polyurethane-acrylate matrix and is tightly combined with the polymer chain segments, filling the pores between the chain segments, making it difficult for water molecules to enter, reducing the affinity with water, and preventing water droplets from wetting the fabric. A large number of pores are still maintained between the fibers and yarns in the fabric, so that the fabric has both good water repellency and air permeability and moisture permeability.
[0035] (2) The present application uses organic silicon-modified titanium dioxide and tetraethyl orthosilicate as precursors and water as solvent to prepare titanium dioxide-modified silica hydrosol, and uses tripropylene glycol diacrylate for secondary modification to obtain silica-modified sol; there is a strong intermolecular force between the silica-modified sol and the polyurethane-acrylate, and the silica plays a role similar to the cross-linking point in the matrix. The inorganic particles and the polymer are connected to form a cross-linking network through chemical bonds, which increases the resistance to bending, rotation, and movement of the molecular chain, hinders the thermal decomposition of the molecular chain, and improves the thermal stability of the coating. The organically modified titanium dioxide and silica of the present application effectively improve the problem that titanium dioxide and silica are directly added as inorganic substances and have no binding force with fabric fibers and have extremely poor washability. Titanium dioxide is filled in the sol-gel of organically modified silane, which not only gives the fabric anti-ultraviolet properties, but also improves its bonding strength with the fabric, enhances durability, improves the wash fastness of the functional layer on the surface of the fabric, and can also obtain good air permeability and soft feel. DETAILED DESCRIPTION
[0036] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Example 1 The preparation method of silicone-modified waterborne polyurethane acrylate emulsion comprises the following steps:
[0038] A1: In a nitrogen atmosphere, 10 g of polyether diol (average molecular weight 1000), 5 g of isophorone diisocyanate, and 0.3 g of dibutyltin dilaurate were added to a reactor, the temperature was controlled at 80°C, and the reaction was kept warm for 1 hour. 1 g of dimethylolpropionic acid and 25 mL of acetone were added, and the reaction was kept warm for 1 hour. The temperature was controlled at 60°C, 5 g of hydroxyethyl methacrylate was added, and the reaction was kept warm for 1 hour. The temperature was controlled at 65°C, and the reaction was kept warm for 1 hour. The temperature was controlled at 35°C, 1.1 g of triethylamine was added, and the reaction was kept warm for 0.5 hour. 30 mL of deionized water was added, and the reaction was kept warm for 1 hour. Acetone was removed by rotary evaporation to obtain an aqueous polyurethane acrylate emulsion;
[0039] A2: In a nitrogen atmosphere, 10 g of nano titanium dioxide, 10 g of 2,4-toluene diisocyanate, and 100 mL of toluene were added into a reaction kettle and dispersed evenly. The temperature was controlled at 80°C, and the mixture was stirred for 6 h. The mixture was washed with anhydrous ethanol and dried to obtain component 1.
[0040] A3: Add 10g of component 1, 15g of γ-aminopropyltriethoxysilane and 100mL of ethyl acetate into a reactor, control the temperature to 50°C, keep the reaction for 3h, add 2mL of anhydrous ethanol to disperse evenly, keep the reaction for 1h, filter and dry to obtain component 2;
[0041] A4: Add 15 mL of anhydrous ethanol, 10 g of component 2, and 12.5 g of tetraethyl orthosilicate into a reaction kettle and disperse them evenly. Add 25 mL of 0.2 mol / L acetic acid solution dropwise. Control the temperature at 25°C and keep the reaction for 6 hours to obtain component 3.
[0042] A5: 1 g of component 3 and 0.6 g of tripropylene glycol diacrylate were added into a reaction kettle and dispersed evenly, and the solvent was removed by vacuum distillation to obtain a silica-modified sol;
[0043] A6: 30 g of aqueous polyurethane acrylate emulsion and 50 g of silica-modified sol were blended to obtain silicone-modified aqueous polyurethane acrylate emulsion.
[0044] Example 2 The preparation method of the silicone-modified waterborne polyurethane acrylate emulsion comprises the following steps:
[0045] A1: In a nitrogen atmosphere, 10 g of polyether diol (average molecular weight 1000), 5 g of isophorone diisocyanate, and 0.3 g of dibutyltin dilaurate were added to a reactor, the temperature was controlled at 80°C, and the reaction was kept warm for 1 hour. 1 g of dimethylolpropionic acid and 25 mL of acetone were added, and the reaction was kept warm for 1 hour. The temperature was controlled at 60°C, 5 g of hydroxyethyl methacrylate was added, and the reaction was kept warm for 1 hour. The temperature was controlled at 65°C, and the reaction was kept warm for 1 hour. The temperature was controlled at 35°C, 1.1 g of triethylamine was added, and the reaction was kept warm for 0.5 hour. 30 mL of deionized water was added, and the reaction was kept warm for 1 hour. Acetone was removed by rotary evaporation to obtain an aqueous polyurethane acrylate emulsion;
[0046] A2: In a nitrogen atmosphere, 10 g of nano titanium dioxide, 12 g of 2,4-toluene diisocyanate, and 200 mL of toluene were added to a reaction kettle and dispersed evenly. The temperature was controlled at 85°C, and the mixture was stirred for 9 h. The mixture was washed with anhydrous ethanol and dried to obtain component 1.
[0047] A3: Add 10g of component 1, 18g of γ-aminopropyltriethoxysilane and 200mL of ethyl acetate into a reactor, control the temperature to 55°C, keep the reaction for 3h, add 10mL of anhydrous ethanol to disperse evenly, keep the reaction for 2h, filter and dry to obtain component 2;
[0048] A4: Add 20 mL of anhydrous ethanol, 10 g of component 2, and 12.5 g of tetraethyl orthosilicate into a reaction kettle and disperse them evenly. Add 20 mL of 0.2 mol / L acetic acid solution dropwise. Control the temperature at 30°C and keep the reaction for 9 hours to obtain component 3.
[0049] A5: 1 g of component 3 and 0.6 g of tripropylene glycol diacrylate were added into a reaction kettle and dispersed evenly, and the solvent was removed by vacuum distillation to obtain a silica-modified sol;
[0050] A6: 30 g of aqueous polyurethane acrylate emulsion and 50 g of silica-modified sol were blended to obtain silicone-modified aqueous polyurethane acrylate emulsion.
[0051] Example 3 The preparation method of silicone-modified waterborne polyurethane acrylate emulsion comprises the following steps:
[0052] A1: In a nitrogen atmosphere, 10 g of polyether diol (average molecular weight 1000), 5 g of isophorone diisocyanate, and 0.3 g of dibutyltin dilaurate were added to a reactor, the temperature was controlled at 80°C, and the reaction was kept warm for 1 hour. 1 g of dimethylolpropionic acid and 25 mL of acetone were added, and the reaction was kept warm for 1 hour. The temperature was controlled at 60°C, 5 g of hydroxyethyl methacrylate was added, and the reaction was kept warm for 1 hour. The temperature was controlled at 65°C, and the reaction was kept warm for 1 hour. The temperature was controlled at 35°C, 1.1 g of triethylamine was added, and the reaction was kept warm for 0.5 hour. 30 mL of deionized water was added, and the reaction was kept warm for 1 hour. Acetone was removed by rotary evaporation to obtain an aqueous polyurethane acrylate emulsion;
[0053] A2: In a nitrogen atmosphere, 10 g of nano titanium dioxide, 15 g of 2,4-toluene diisocyanate, and 300 mL of toluene were added to a reaction kettle and dispersed evenly. The temperature was controlled at 90°C, and the mixture was stirred for 12 h. The mixture was washed with anhydrous ethanol and dried to obtain component 1.
[0054] A3: Add 10g of component 1, 20g of γ-aminopropyltriethoxysilane and 300mL of ethyl acetate into a reactor, control the temperature at 60°C, keep the reaction for 6h, add 20mL of anhydrous ethanol to disperse evenly, keep the reaction for 3h, filter and dry to obtain component 2;
[0055] A4: Add 25 mL of anhydrous ethanol, 10 g of component 2, and 12.5 g of tetraethyl orthosilicate into a reaction kettle and disperse them evenly. Add 25 mL of 0.2 mol / L acetic acid solution dropwise. Control the temperature at 35°C and keep the reaction for 12 hours to obtain component 3.
[0056] A5: 1 g of component three and 0.6 g of tripropylene glycol diacrylate were added into a reaction kettle and dispersed evenly. The solvent was removed by distillation under reduced pressure to obtain a silica-modified sol.
[0057] A6: 30 g of aqueous polyurethane acrylate emulsion and 50 g of silica-modified sol were blended to obtain silicone-modified aqueous polyurethane acrylate emulsion.
[0058] Embodiment 4 The preparation method of the coating composition comprises the following steps:
[0059] A1: Clean the dispersion tank, add 80 parts by weight of the silicone-modified waterborne polyurethane acrylate emulsion prepared in Example 1 and 10 parts by weight of an anti-ultraviolet additive (Huntsman model UV-FAST N2) into the tank, stir at 200-300 rpm for 10 min, and mix and disperse evenly to form a premix;
[0060] A2: Add 0.2 parts by weight of dispersant (sodium polyacrylate, model BG554 produced by Dongguan Bogao Chemical Co., Ltd.), 0.5 parts by weight of defoamer (model LLT-DF-723 produced by Xinxiang Longlidian Chemical Preparation Co., Ltd.), 2 parts by weight of humectant (propylene glycol), 5 parts by weight of aqueous wax emulsion feel agent (model ENCOR7605 produced by Jining Huakai Resin Co., Ltd.), and 0.3 parts by weight of ammonia pH regulator to the premix while stirring, and stir at 400 rpm for 20 min;
[0061] A3: 3 parts by weight of thickener PTF was added, and the mixture was stirred and dispersed at 600 rpm for 20 minutes to obtain a coating composition.
[0062] Compared with Example 4, Example 5 only replaces the silicone-modified waterborne polyurethane acrylate emulsion prepared in Example 1 added in Example 4 with an equal amount of the silicone-modified waterborne polyurethane acrylate emulsion prepared in Example 2, and its components and preparation method are exactly the same as those of Example 4.
[0063] Compared with Example 4, Example 6 only replaces the silicone-modified waterborne polyurethane acrylate emulsion prepared in Example 1 added in Example 4 with an equal amount of the silicone-modified waterborne polyurethane acrylate emulsion prepared in Example 3, and its components and preparation method are exactly the same as those of Example 4.
[0064] Comparative Example 1 The preparation method of the silicone-modified waterborne polyurethane acrylate emulsion comprises the following steps:
[0065] A1: In a nitrogen atmosphere, 10 g of polyether diol (average molecular weight 1000), 5 g of isophorone diisocyanate, and 0.3 g of dibutyltin dilaurate were added to a reactor, the temperature was controlled at 80°C, and the reaction was kept warm for 1 hour. 1 g of dimethylolpropionic acid and 25 mL of acetone were added, and the reaction was kept warm for 1 hour. The temperature was controlled at 60°C, 5 g of hydroxyethyl methacrylate was added, and the reaction was kept warm for 1 hour. The temperature was controlled at 65°C, and the reaction was kept warm for 1 hour. The temperature was controlled at 35°C, 1.1 g of triethylamine was added, and the reaction was kept warm for 0.5 hour. 30 mL of deionized water was added, and the reaction was kept warm for 1 hour. Acetone was removed by rotary evaporation to obtain an aqueous polyurethane acrylate emulsion;
[0066] A2: In a nitrogen atmosphere, 10 g of nano titanium dioxide, 10 g of 2,4-toluene diisocyanate, and 100 mL of toluene were added into a reaction kettle and dispersed evenly. The temperature was controlled at 80°C, and the mixture was stirred for 6 h. The mixture was washed with anhydrous ethanol and dried to obtain component 1.
[0067] A3: Add 10g of component 1, 15g of γ-aminopropyltriethoxysilane and 100mL of ethyl acetate into a reactor, control the temperature to 50°C, keep the reaction for 3h, add 2mL of anhydrous ethanol to disperse evenly, keep the reaction for 1h, filter and dry to obtain component 2;
[0068] A4: Add 15 mL of anhydrous ethanol and 12.5 g of tetraethyl orthosilicate into a reaction kettle and disperse them evenly. Add 25 mL of 0.2 mol / L acetic acid solution dropwise. Control the temperature at 25°C and keep the reaction for 6 hours. Filter and dry. Add 10 g of component 2 to obtain component 3.
[0069] A5: 1 g of component three and 0.6 g of tripropylene glycol diacrylate were added into a reaction kettle and dispersed evenly. The solvent was removed by distillation under reduced pressure to obtain a silica-modified sol.
[0070] A6: 30 g of aqueous polyurethane acrylate emulsion and 50 g of silica-modified sol were blended to obtain silicone-modified aqueous polyurethane acrylate emulsion.
[0071] Comparative Example 2 The preparation method of silicone-modified waterborne polyurethane acrylate emulsion comprises the following steps:
[0072] A1: In a nitrogen atmosphere, 10 g of polyether diol (average molecular weight 1000), 5 g of isophorone diisocyanate, and 0.3 g of dibutyltin dilaurate were added to a reactor, the temperature was controlled at 80°C, and the reaction was kept warm for 1 hour. 1 g of dimethylolpropionic acid and 25 mL of acetone were added, and the reaction was kept warm for 1 hour. The temperature was controlled at 60°C, 5 g of hydroxyethyl methacrylate was added, and the reaction was kept warm for 1 hour. The temperature was controlled at 65°C, and the reaction was kept warm for 1 hour. The temperature was controlled at 35°C, 1.1 g of triethylamine was added, and the reaction was kept warm for 0.5 hour. 30 mL of deionized water was added, and the reaction was kept warm for 1 hour. Acetone was removed by rotary evaporation to obtain an aqueous polyurethane acrylate emulsion;
[0073] A2: In a nitrogen atmosphere, 10 g of nano titanium dioxide, 10 g of 2,4-toluene diisocyanate, and 100 mL of toluene were added into a reaction kettle and dispersed evenly. The temperature was controlled at 80°C, and the mixture was stirred for 6 h. The mixture was washed with anhydrous ethanol and dried to obtain component 1.
[0074] A3: Add 10g of component 1, 15g of γ-aminopropyltriethoxysilane and 100mL of ethyl acetate into a reactor, control the temperature to 50°C, keep the reaction for 3h, add 2mL of anhydrous ethanol to disperse evenly, keep the reaction for 1h, filter and dry to obtain component 2;
[0075] A4: 15 mL of anhydrous ethanol and 12.5 g of tetraethyl orthosilicate were added to a reaction kettle and dispersed evenly, 25 mL of 0.2 mol / L acetic acid solution was added dropwise, the temperature was controlled at 25°C, the reaction was kept warm for 6 h, filtered, dried, and 10 g of component 2 was added to obtain a silica-modified sol;
[0076] A5: 30 g of aqueous polyurethane acrylate emulsion and 50 g of silica-modified sol were blended to obtain silicone-modified aqueous polyurethane acrylate emulsion.
[0077] Comparative Example 3 The preparation method of silicone-modified water-based polyurethane acrylate emulsion comprises the following steps:
[0078] A1: In a nitrogen atmosphere, 10 g of polyether diol (average molecular weight 1000), 5 g of isophorone diisocyanate, and 0.3 g of dibutyltin dilaurate were added to a reactor, the temperature was controlled at 80°C, and the reaction was kept warm for 1 hour. 1 g of dimethylolpropionic acid and 25 mL of acetone were added, and the reaction was kept warm for 1 hour. The temperature was controlled at 60°C, 5 g of hydroxyethyl methacrylate was added, and the reaction was kept warm for 1 hour. The temperature was controlled at 65°C, and the reaction was kept warm for 1 hour. The temperature was controlled at 35°C, 1.1 g of triethylamine was added, and the reaction was kept warm for 0.5 hour. 30 mL of deionized water was added, and the reaction was kept warm for 1 hour. Acetone was removed by rotary evaporation to obtain an aqueous polyurethane acrylate emulsion;
[0079] A2: In a nitrogen atmosphere, 10 g of nano titanium dioxide, 10 g of 2,4-toluene diisocyanate, and 100 mL of toluene were added into a reaction kettle and dispersed evenly. The temperature was controlled at 80°C, and the mixture was stirred for 6 h. The mixture was washed with anhydrous ethanol and dried to obtain component 1.
[0080] A3: Add 15 mL of anhydrous ethanol and 12.5 g of tetraethyl orthosilicate into a reaction kettle and disperse them evenly. Add 25 mL of 0.2 mol / L acetic acid solution dropwise. Control the temperature at 25°C and keep the reaction for 6 hours. Filter and dry. Add 10 g of component 1 to obtain component 3.
[0081] A4: 1 g of component three and 0.6 g of tripropylene glycol diacrylate were added into a reaction kettle and dispersed evenly. The solvent was removed by distillation under reduced pressure to obtain a silica-modified sol.
[0082] A5: 30 g of aqueous polyurethane acrylate emulsion and 50 g of silica-modified sol were blended to obtain silicone-modified aqueous polyurethane acrylate emulsion.
[0083] Compared with Example 4, Comparative Example 4 only replaces the silicone-modified waterborne polyurethane acrylate emulsion prepared in Example 1 added in Example 4 with an equal amount of the silicone-modified waterborne polyurethane acrylate emulsion prepared in Comparative Example 1, and its components and preparation method are completely consistent with those of Example 4.
[0084] Compared with Example 4, Comparative Example 5 only replaces the silicone-modified waterborne polyurethane acrylate emulsion prepared in Example 1 added in Example 4 with an equal amount of the silicone-modified waterborne polyurethane acrylate emulsion prepared in Comparative Example 2, and its components and preparation method are completely consistent with those of Example 4.
[0085] Compared with Example 4, Comparative Example 6 only replaces the silicone-modified waterborne polyurethane acrylate emulsion prepared in Example 1 added in Example 4 with an equal amount of the silicone-modified waterborne polyurethane acrylate emulsion prepared in Comparative Example 3, and its components and preparation method are exactly the same as those of Example 4.
[0086] Performance Testing
[0087] Preparation of samples: Printing process: The coating compositions prepared in Examples 4-6 and Comparative Examples 4-6 were used as printing pastes; 100% printing paste was directly printed (recommended mesh: 800 mesh), dried with hot air, and baked at 150° C. for 3 min to obtain a fabric with sunscreen and water repellent effects;
[0088] (1) Ultraviolet protection factor: tested in accordance with GB / T 18830-2009 “Evaluation of UV protection performance of textiles”. The test results are shown in Table 2.
[0089] (2) Water repellency: The test was conducted according to GB / T 4745-2012 “Test for Determination of Surface Wetting Resistance of Textile Fabrics - Water Splashing Test”. The water repellency level of the samples was differentiated according to the water repellency level standard in Table 1. The test results are shown in Table 2.
[0090] Table 1: Water repellency rating standards
[0091] Level 1 Wetting of all the exposed surfaces Level 2 Half of the shower surface is wet Level 3 The showered surface is only wetted in a small area without any connection Level 4 The showered surface is not wet, but has small water droplets on it. Level 5 The showered surface is not wet and there are no small water droplets on the surface
[0092] (3) Color fastness to washing: tested according to GB / T 3921.1-2008 “Textiles - Tests for Color Fastness - Color Fastness to Washing”. The test results are shown in Table 2.
[0093] (4) Water vapor permeability: measured according to the water vapor permeability cup method: Method A of GB / T 12704-1991 "Test method for water vapor permeability of fabrics". The test results are shown in Table 3 and Table 2.
[0094] Table 2: Statistical table of performance test data of Examples 4-6 and Comparative Examples 4-6
[0095]
[0096] As shown in Table 2, the coating composition prepared in the present application, as a finishing agent, gives the fabric excellent water repellency and UV resistance, and after multiple washings, the water repellency still reaches level 4 or above, and the UPF level still remains at 50. + The coating composition prepared in the present application is applied to fabrics, which not only imparts excellent water repellency and UV resistance to the fabrics, but also does not affect the moisture permeability of the fabrics themselves.
[0097] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A coating composition having sunscreen and water repellent function, characterized in that: The method comprises the following raw materials in parts by weight: 50-80 parts of silicone-modified waterborne polyurethane acrylate emulsion, 10-25 parts of UV protection additive, 8 parts of additive, and 1-3 parts of thickener PTF; The preparation method of the silicone-modified waterborne polyurethane acrylate emulsion comprises the following steps: A1: In a nitrogen atmosphere, polyether diol, isophorone diisocyanate and dibutyltin dilaurate are added to a reaction kettle, the temperature is controlled at 80-90°C, and the reaction is kept warm for 1-3h. Dimethylolpropionic acid and acetone are added, and the reaction is kept warm for 1-3h. The temperature is controlled at 60-70°C. Hydroxyethyl methacrylate is added, and the reaction is kept warm for 1-3h. The temperature is controlled at 65-75°C, and the reaction is kept warm for 1-3h. The temperature is controlled at 35-45°C, triethylamine is added, and the reaction is kept warm for 0.5-1h. Deionized water is added, and the reaction is kept warm for 1-3h. Acetone is removed by rotary evaporation to obtain an aqueous polyurethane acrylate emulsion; A2: blending an aqueous polyurethane acrylate emulsion and a silica-modified sol to obtain an organosilicon-modified aqueous polyurethane acrylate emulsion; The preparation method of the silica modified sol comprises the following steps: S1: In a nitrogen atmosphere, nano titanium dioxide, 2,4-toluene diisocyanate and toluene are added into a reaction kettle and dispersed evenly, the temperature is controlled at 80-90°C, the mixture is stirred for 6-12 hours, washed with anhydrous ethanol and dried to obtain component 1; S2: Add component 1, γ-aminopropyltriethoxysilane and ethyl acetate into a reaction kettle, control the temperature at 50-60°C, keep the temperature for reaction for 3-6 hours, add anhydrous ethanol to disperse evenly, keep the temperature for reaction for 1-3 hours, filter and dry to obtain component 2; S3: Add anhydrous ethanol, component 2, and tetraethyl orthosilicate into a reaction kettle and disperse them evenly, dropwise add acetic acid solution, control the temperature at 25-35°C, and keep the reaction warm for 6-12 hours to obtain component 3; S4: Add components three and tripropylene glycol diacrylate into a reaction kettle and disperse them evenly, and remove the solvent by distillation under reduced pressure to obtain a silica-modified sol.
2. A coating composition having sunscreen and water repellent function according to claim 1, characterized in that: The addition ratio of polyether diol, isophorone diisocyanate, dibutyltin dilaurate, dihydroxymethylpropionic acid, acetone, hydroxyethyl methacrylate, triethylamine and deionized water in A1 is 10g: 5-8g: 0.3-0.4g: 1-2g: 25-50mL: 5-8g: 1.1-1.5g: 30-60mL.
3. A coating composition with sunscreen and water repellent function according to claim 1, characterized in that: The mass ratio of the aqueous polyurethane acrylate emulsion and the silica-modified sol in A2 is 20-30:20-50.
4. A coating composition with sunscreen and water repellent function according to claim 1, characterized in that: The addition ratio of nano-titanium dioxide, 2,4-toluene diisocyanate and toluene in S1 is 10g: 10-15g: 100-300mL.
5. The coating composition with sunscreen and water repellent function according to claim 1, characterized in that: The addition ratio of component 1, γ-aminopropyltriethoxysilane, ethyl acetate, and anhydrous ethanol in S2 is 10 g: 15-20 g: 100-300 mL: 2-20 mL.
6. A coating composition with sunscreen and water repellent function according to claim 1, characterized in that: The acetic acid solution in S3 is 0.2-0.3 mol / L acetic acid solution, and the addition ratio of anhydrous ethanol, component two, tetraethyl orthosilicate, and acetic acid solution is 15-25 mL: 10 g: 4-12.5 g: 10-25 mL.
7. A coating composition with sunscreen and water repellent function according to claim 1, characterized in that: The mass ratio of component three and tripropylene glycol diacrylate in S4 is 1:0.3-0.
6.
8. The coating composition with sunscreen and water repellent function according to claim 1, characterized in that: The anti-ultraviolet additive is a benzotriazole ultraviolet absorber.
9. The coating composition with sunscreen and water repellent function according to claim 1, characterized in that: The auxiliary agent includes 0.2-0.5 parts of dispersant, 0.5-1 parts of defoamer, 2-4 parts of moisturizer, 5-8 parts of water-based wax emulsion feel agent, and 0.3-0.5 parts of pH regulator.