Anode aluminum foil for aluminum electrolytic capacitor and preparation method thereof

By adding zinc ions and using aniline polymer corrosion inhibitors in the pretreatment of aluminum foil, combined with anodizing treatment, the problems of high specific capacitance and water resistance of anode aluminum foil for aluminum electrolytic capacitors were solved, and the performance was significantly improved.

CN118299186BActive Publication Date: 2024-11-05YUSHENG (GUANGDONG) ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410543304.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-05
Publication Date
2024-11-05
Estimated Expiration
2044-05-05

AI Technical Summary

Technical Problem

The performance improvement of existing aluminum foil anodes for aluminum electrolytic capacitors is insufficient to simultaneously meet the requirements of high specific capacitance and good water resistance.

Method used

By adding zinc ions during pretreatment for chemical zinc plating, combining aniline polymers as corrosion inhibitors, and performing anodizing after pore-expanding corrosion, a high-quality oxide film is formed, improving the pore uniformity and corrosion resistance of aluminum foil.

Benefits of technology

It improves the specific capacitance and water resistance of the anode aluminum foil used in aluminum electrolytic capacitors, reduces corrosion resistance, promotes the formation of tunnel pores, reduces the phenomenon of parallel pores, and enhances the performance of the capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004821644690000081
    Figure BDA0004821644690000081
  • Figure BDA0004821644690000091
    Figure BDA0004821644690000091
Patent Text Reader

Abstract

The present invention relates to the technical field of capacitors, specifically to an anode aluminum foil for aluminum electrolytic capacitors and a preparation method thereof, comprising the following processes: pre-treating the aluminum foil, pore corrosion, pore expansion corrosion, and post-treatment in sequence to obtain the anode aluminum foil; the pre-treatment uses an alkaline solution containing zinc ions to deposit elemental zinc on the surface of the aluminum foil. The present application adds zinc ions to an alkaline solution, chemically zinc-plating the aluminum foil, dissolving aluminum and its oxide film while the zinc ions are replaced with aluminum, and elemental zinc is uniformly and dispersedly deposited on its surface, and a zinc-aluminum micro-battery can be formed in pore corrosion, wherein zinc is a positive electrode and aluminum is a negative electrode, which can increase the current density in the electrolytic circuit to a certain extent, reduce corrosion resistance, accelerate the corrosion rate of aluminum, promote the generation of tunnel holes, and reduce the phenomenon of pores; and the presence of the micro-battery unit can also improve the pore density and pore uniformity of the aluminum foil, which helps to increase the specific capacitance of the anode aluminum foil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of capacitors, and in particular to an anode aluminum foil for aluminum electrolytic capacitors and a preparation method thereof. Background Art

[0002] Electrolytic capacitors are one of the indispensable components in electronic products. As a common electronic device, aluminum electrolytic capacitors have the characteristics of excellent performance, large capacity, low price, easy processing, and convenient use. They have high capacitance values ​​and low impedance at low frequencies. They are widely used in electronic products such as information electronic equipment, instruments and meters, electromechanical equipment, and household appliances. The anode of an aluminum electrolytic capacitor is made of pure aluminum foil that has been etched on the surface and then oxidized to form on the surface. The anode aluminum foil for aluminum electrolytic capacitors is a key material and has an important influence on its performance. Therefore, we propose an anode aluminum foil for aluminum electrolytic capacitors and a preparation method thereof. Summary of the invention

[0003] The object of the present invention is to provide an anode aluminum foil for aluminum electrolytic capacitors and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing an anode aluminum foil for an aluminum electrolytic capacitor, comprising the following processes: subjecting the aluminum foil to pretreatment, pore formation corrosion, pore expansion corrosion, and post-treatment in sequence to obtain an anode aluminum foil.

[0005] Furthermore, the pretreatment process is as follows: placing the aluminum foil in an alkaline solution at 40 to 45° C. for 20 to 60 seconds.

[0006] Furthermore, the alkaline solution is obtained by dissolving zinc oxide with 5% to 7% sodium hydroxide; the amount of zinc oxide added to the alkaline solution is 0.9 to 1.3 wt%.

[0007] In the above technical solution, the alkaline solution used in the pretreatment can remove the oxide film and oil film on the surface of the aluminum foil, and evenly clean the dirt and excessively thick oxide film on the surface of the aluminum foil, which is helpful to improve the penetration of chloride ions and the breakdown of the oxide film in the subsequent pitting corrosion process, thereby promoting the reaction of chloride ions with the aluminum foil matrix to form a soluble complex, which is further corroded to generate a hydrolyzable complex, promote the start of pitting corrosion, improve the pore quality of the aluminum foil, and improve its porosity and pore uniformity. Zinc oxide is added to sodium hydroxide and dissolved to obtain an alkaline solution containing zinc ions, and the aluminum foil is chemically zinc-plated. While dissolving aluminum and its oxide film, zinc ions are replaced with aluminum, and elemental zinc is uniformly and dispersedly deposited on its surface.

[0008] Furthermore, the pore etching process is as follows: the aluminum foil obtained after pretreatment is used as an anode, and graphite is used as a cathode, and electrolyzed in a pore-forming solution at a temperature of 60 to 80° C. for 90 to 150 seconds with a current density of 0.15 to 0.20 A / cm2;

[0009] The pore-forming solution includes the following components (in molar concentration): 1 M hydrochloric acid, 1-3 M sulfuric acid and 0.2-0.3 M sodium nitrate.

[0010] In the above technical scheme, hydrochloric acid-sulfuric acid-nitric acid is used as the electrolyte system, two parallel graphite electrode plates are used as cathodes, and the pretreated aluminum foil is used as the anode for electrolytic corrosion to form pores. The pore corrosion causes pitting on the surface of the aluminum foil through the reaction of chloride ions in the pore solution with the metal aluminum and its oxide film, and further develops the pitting behavior, ensuring the density of the pores and the uniformity of the pore depth. The surface of the pretreated aluminum foil contains elemental zinc, and a zinc-aluminum micro-battery is formed in the pore corrosion, in which zinc is the positive electrode and aluminum is the negative electrode, which can increase the current density in the electrolytic circuit to a certain extent, reduce corrosion resistance, accelerate the corrosion rate of aluminum, promote the formation of tunnel pores, and reduce the phenomenon of pores; and the presence of the micro-battery unit can also improve the pore density and pore uniformity of the aluminum foil, which helps to increase the specific capacitance of the anode aluminum foil.

[0011] Furthermore, the hole expansion etching process is as follows: the aluminum foil obtained after the hole expansion etching is used as the anode and the graphite is used as the cathode, and electrolysis is performed in the hole expansion liquid at a temperature of 70 to 80° C. for 360 to 600 seconds with a current density of 0.08 to 0.12 A / cm2;

[0012] Then, it is washed with 0.25-0.30M nitric acid at a temperature of 30-35°C and dried at 120-150°C.

[0013] Further, the pore enlarging solution includes the following components: 1-2M hydrochloric acid, 0.4-1.0g / L corrosion inhibitor;

[0014] The corrosion inhibitor is a mixture of one or more of polyethylene glycol, polyacrylic acid, ethylene glycol, aniline, sodium hexametaphosphate, sodium dodecylbenzene sulfonate and aniline polymer.

[0015] Further, the aniline polymer is prepared by the following process:

[0016] In an argon atmosphere, 4-vinylaniline, maleic anhydride, azobisisobutyronitrile and 2-phenyl-2-propylbenzodisulfide are mixed, stirred and reacted at 60-70°C for 12-15 hours to obtain a polymer; rotary evaporation, methanol precipitation, centrifugation and purification;

[0017] Deionized water was added and mixed, and the pH value was adjusted to 4.0-4.5 with hydrochloric acid. The mixture was stirred and reacted at 60-70° C. for 120-150 minutes. The mixture was dried to obtain an aniline polymer.

[0018] Further, the aniline polymer is prepared from the following molar components: 3 to 4 parts of 4-vinylaniline, 1 to 2 parts of maleic anhydride, 6 to 9 parts of 2-phenyl-2-propylbenzodisulfide, and 0.14 to 0.21 parts of azobisisobutyronitrile;

[0019] The ratio of polymer to deionized water is 50 g / 100 mL.

[0020] In the above technical scheme, hydrochloric acid is used as a pore expansion liquid to further electrolytically etch the aluminum foil to expand the tunnel holes formed after the pore corrosion, ensure that the etched holes have a certain aperture, avoid the blockage of the oxide film grown in the post-treatment process, and cause the reduction of the specific surface area of ​​the aluminum foil, affecting the improvement of the specific capacitance of the anode aluminum foil. Aniline polymer is added to the pore expansion liquid as a corrosion inhibitor to form a slow-release layer on the surface of the aluminum foil, making it easy for corrosion to occur at the original pitting, which is conducive to the orderly increase and deepening of the etched holes, and reducing the occurrence of string holes and parallel holes.

[0021] The aniline polymer is obtained by chain polymerization and hydrolysis of 4-vinylaniline, maleic anhydride, and 2-phenyl-2-propylbenzodisulfide to form a linear polymer. The polymer has good dispersibility in the pore expansion liquid and can be evenly distributed on the surface of the aluminum foil, thereby reducing its self-corrosion effect, alleviating the uneven thickness and distribution of the polymer caused by electropolymerization after the addition of the aniline monomer, promoting the growth of the tunnel hole, and improving the tunnel hole.

[0022] Then, it is washed with nitric acid and dried at a relatively low temperature to remove residual chloride ions Cl- in the pores, prevent the removal of structural water, reduce hydration, and avoid affecting the formation of the oxide film.

[0023] Further, the post-processing process is as follows:

[0024] The aluminum foil obtained after hole expansion and corrosion is placed in a boric acid solution for anodization at a voltage of 520 to 720 V for 12 to 20 minutes;

[0025] The aluminum foil is immersed in a stearic acid solution at 75 to 85° C. for 20 to 30 minutes; and dried at 120 to 150° C. to obtain an anode aluminum foil.

[0026] The mass concentration of the boric acid solution is 13% to 17%, and it contains ammonium pentaborate and boric acid in a mass ratio of (1 to 3):10;

[0027] The mass concentration of the stearic acid solution is 100%.

[0028] In the above technical scheme, an oxide film is formed on the surface of the aluminum foil after hole expansion corrosion through anodization in the post-treatment process, and then it is modified by stearic acid, and its surface energy is reduced by stearic acid, and its hydrophobicity is improved, which can effectively improve the corrosion resistance and hydration resistance of the anode aluminum foil; the aluminum oxide insulating layer as the dielectric of the aluminum electrolytic capacitor is dried at a lower temperature, which can prevent the removal of structural water, reduce hydration, and avoid affecting the quality of the oxide film.

[0029] Furthermore, the aluminum foil is electronic aluminum foil (plain foil) with a thickness of 20 to 100 μm, a purity of more than 99.99%, and a

[100] crystal plane occupancy of more than 98%.

[0030] In the above technical scheme, an aluminum foil with a higher

[100] crystal plane occupancy rate is selected as the raw material. The surface energy of the crystal plane is lower, so that there are more potential corrosion holes on the surface of the aluminum foil, which are first corroded in the pore corrosion and first covered by the corrosion inhibitor in the pore expansion corrosion, thereby promoting the corrosion of the

[124] and other crystal planes, so that the corrosion holes continue to expand downward, the formation and growth of tunnel holes are promoted, the merging hole phenomenon is alleviated, the corrosion hole density is maintained, and it is helpful to improve the specific capacitance of the anode aluminum foil.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] The present invention discloses an anode aluminum foil for aluminum electrolytic capacitors and a preparation method thereof. Zinc ions are added to an alkaline solution used in pretreatment to chemically zinc-plate the aluminum foil. While dissolving aluminum and its oxide film, zinc ions are replaced with aluminum, and elemental zinc is uniformly and dispersedly deposited on the surface of the aluminum foil. A zinc-aluminum microbattery can be formed in pore corrosion, wherein zinc is a positive electrode and aluminum is a negative electrode. The current density in the electrolytic circuit can be increased to a certain extent, the corrosion resistance can be reduced, the corrosion rate of aluminum can be accelerated, the formation of tunnel holes can be promoted, and the pore-joining phenomenon can be reduced. The presence of the microbattery unit can also improve the pore density and pore uniformity of the aluminum foil, which is helpful to increase the specific capacitance of the anode aluminum foil. DETAILED DESCRIPTION

[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] In the following specific implementations,

[0035] Aluminum foil: high-purity aluminum foil with a thickness of 100 μm, the mass fraction of aluminum is greater than 99.99%, and the

[100] crystal plane occupancy is greater than 98%.

[0036] Polyacrylic acid: P434403, average weight average molecular weight 2000, from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0037] Embodiment 1: A method for preparing an anode aluminum foil for an aluminum electrolytic capacitor, comprising the following process:

[0038] Step (1) pretreatment: zinc oxide is mixed with 5% sodium hydroxide solution, stirred and dissolved to obtain an alkaline solution, wherein the amount of zinc oxide added is 0.9 wt %; aluminum foil is placed in the alkaline solution at 40° C. and treated for 20 seconds;

[0039] Step (2) Pore etching: The aluminum foil obtained after pretreatment is used as the anode and graphite is used as the cathode. Electrolysis is carried out in the porolysis solution at 60°C for 150s with a current density of 0.20A / cm 2 The pore-forming solution includes the following components: 1M hydrochloric acid, 1M sulfuric acid and 0.2M sodium nitrate;

[0040] Step (3) hole expansion corrosion:

[0041] The aluminum foil obtained after pore etching was used as the anode and graphite as the cathode. The aluminum foil was electrolyzed in the pore expansion solution at 70°C for 360s with a current density of 0.12A / cm2. The aluminum foil was then washed with 0.25M nitric acid at 30°C and dried at 120°C.

[0042] The pore-enlarging liquid includes the following components: 1M hydrochloric acid, 0.4g / L corrosion inhibitor aniline polymer; the aniline polymer is prepared by the following process: in an argon atmosphere, 4-vinyl aniline, maleic anhydride, azobisisobutyronitrile, and 2-phenyl-2-propylbenzodisulfide are mixed, stirred at 60°C for 12 hours to obtain a polymer; rotary evaporation, methanol precipitation, centrifugation, purification; deionized water is added to mix, hydrochloric acid is used to adjust the pH to 4.0, and stirred at 60°C for 120 minutes; drying is performed to obtain an aniline polymer; the aniline polymer is prepared by the following molar components: 3 parts of 4-vinyl aniline, 1 part of maleic anhydride, 6 parts of 2-phenyl-2-propylbenzodisulfide, and 0.14 parts of azobisisobutyronitrile; the ratio of polymer to deionized water is 50g / 100mL;

[0043] Step (4) post-processing:

[0044] The aluminum foil obtained after hole expansion corrosion is placed in a boric acid solution for anodization at a voltage of 520V for 20 minutes; it is immersed in a 100% stearic acid solution at 75°C for 20 minutes; and it is dried at 120°C to obtain an anode aluminum foil; the mass concentration of the boric acid solution is 13%, and it contains ammonium pentaborate and boric acid in a mass ratio of 1:10.

[0045] Embodiment 2: A method for preparing an anode aluminum foil for an aluminum electrolytic capacitor, comprising the following process:

[0046] Step (1) pretreatment: zinc oxide is mixed with 6% sodium hydroxide solution, stirred and dissolved to obtain an alkaline solution, wherein the amount of zinc oxide added is 1.0 wt %; aluminum foil is placed in the alkaline solution at 42° C. and treated for 40 seconds;

[0047] Step (2) Pore formation corrosion: The aluminum foil obtained after pretreatment is used as the anode and the graphite is used as the cathode. Electrolysis is carried out in the pore formation solution at 70°C for 120s with a current density of 0.18A / cm 2 The pore-forming solution includes the following components: 1M hydrochloric acid, 2M sulfuric acid and 0.25M sodium nitrate;

[0048] Step (3) hole expansion corrosion:

[0049] The aluminum foil obtained after pore etching was used as the anode and graphite as the cathode. The aluminum foil was electrolyzed in the pore expansion solution at 75°C for 480s with a current density of 0.10A / cm2. The aluminum foil was then washed with 0.27M nitric acid at 32°C and dried at 135°C.

[0050] The pore-enlarging liquid includes the following components: 1.5M hydrochloric acid, 0.7 / L corrosion inhibitor aniline polymer; the aniline polymer is prepared by the following process: in an argon atmosphere, 4-vinyl aniline, maleic anhydride, azobisisobutyronitrile, and 2-phenyl-2-propylbenzodisulfide are mixed, and the mixture is stirred at 65°C for 13 hours to obtain a polymer; rotary evaporation, methanol precipitation, centrifugation, and purification; deionized water is added to mix, hydrochloric acid is used to adjust the pH to 4.2, and the mixture is stirred at 65°C for 135 minutes; drying is performed to obtain an aniline polymer; the aniline polymer is prepared by the following molar components: 3.5 parts of 4-vinyl aniline, 1.5 parts of maleic anhydride, 7.5 parts of 2-phenyl-2-propylbenzodisulfide, and 0.18 parts of azobisisobutyronitrile; the ratio of the polymer to the deionized water is 50g / 100mL;

[0051] Step (4) post-processing:

[0052] The aluminum foil obtained after hole expansion corrosion was placed in a boric acid solution for anodization at a voltage of 620V and a power-on time of 16 minutes; it was immersed in a 100% stearic acid solution at 80°C for 25 minutes; and it was dried at a temperature of 135°C to obtain an anode aluminum foil; the mass concentration of the boric acid solution was 15%, and it contained ammonium pentaborate and boric acid in a mass ratio of 2:10.

[0053] Embodiment 3: A method for preparing an anode aluminum foil for an aluminum electrolytic capacitor, comprising the following process:

[0054] Step (1) pretreatment: zinc oxide is mixed with 7% sodium hydroxide solution, stirred and dissolved to obtain an alkaline solution, wherein the amount of zinc oxide added is 1.3 wt %; aluminum foil is placed in the alkaline solution at 45° C. and treated for 60 seconds;

[0055] Step (2) Pore formation corrosion: The aluminum foil obtained after pretreatment is used as the anode and graphite is used as the cathode. Electrolysis is carried out in the porolysis solution at 80°C for 150s with a current density of 0.15A / cm 2 The pore-forming solution includes the following components: 1M hydrochloric acid, 3M sulfuric acid and 0.3M sodium nitrate;

[0056] Step (3) hole expansion corrosion:

[0057] The aluminum foil obtained after pore etching was used as the anode and graphite as the cathode in the pore expansion solution at 80°C for 600s with a current density of 0.08A / cm2; then, it was washed with 0.30M nitric acid at 35°C and dried at 150°C;

[0058] The pore-enlarging liquid includes the following components: 2M hydrochloric acid, 1.0g / L corrosion inhibitor aniline polymer; the aniline polymer is prepared by the following process: in an argon atmosphere, 4-vinylaniline, maleic anhydride, azobisisobutyronitrile, and 2-phenyl-2-propylbenzodisulfide are mixed, stirred at 70°C for 15 hours to obtain a polymer; rotary evaporation, methanol precipitation, centrifugation, purification; deionized water is added to mix, hydrochloric acid is used to adjust the pH to 4.5, and stirred at 70°C for 150 minutes; drying is performed to obtain an aniline polymer; the aniline polymer is prepared by the following molar components: 4 parts of 4-vinylaniline, 2 parts of maleic anhydride, 9 parts of 2-phenyl-2-propylbenzodisulfide, and 0.21 parts of azobisisobutyronitrile; the ratio of polymer to deionized water is 50g / 100mL;

[0059] Step (4) post-processing:

[0060] The aluminum foil obtained after hole expansion corrosion was placed in a boric acid solution for anodization at a voltage of 720V for 12 minutes; placed in a 100% stearic acid solution at 85°C for 30 minutes; dried at 150°C to obtain an anode aluminum foil; the mass concentration of the boric acid solution was 17%, and contained ammonium pentaborate and boric acid in a mass ratio of 3:10.

[0061] Comparative Example 1: A method for preparing an anode aluminum foil for an aluminum electrolytic capacitor, comprising the following processes:

[0062] Step (1) pretreatment: zinc oxide is mixed with 5% sodium hydroxide solution, stirred and dissolved to obtain an alkaline solution, wherein the amount of zinc oxide added is 0.9 wt %; aluminum foil is placed in the alkaline solution at 40° C. and treated for 20 seconds;

[0063] Step (2) Pore etching: The aluminum foil obtained after pretreatment is used as the anode and graphite is used as the cathode. Electrolysis is carried out in the porolysis solution at 60°C for 150s with a current density of 0.20A / cm 2 The pore-forming solution includes the following components: 1M hydrochloric acid, 1M sulfuric acid and 0.2M sodium nitrate;

[0064] Step (3) hole expansion corrosion:

[0065] The aluminum foil obtained after pore corrosion was used as the anode and graphite as the cathode. The aluminum foil was electrolyzed in the pore expansion solution at 70°C for 360s with a current density of 0.12A / cm2. The aluminum foil was then washed with 0.25M nitric acid at 30°C and dried at 120°C. The pore expansion solution included the following components: 1M hydrochloric acid and 0.4g / L corrosion inhibitor aniline.

[0066] Step (4) post-processing:

[0067] The aluminum foil obtained after hole expansion corrosion is placed in a boric acid solution for anodization at a voltage of 520V for 20 minutes; it is immersed in a 100% stearic acid solution at 75°C for 20 minutes; and it is dried at 120°C to obtain an anode aluminum foil; the mass concentration of the boric acid solution is 13%, and it contains ammonium pentaborate and boric acid in a mass ratio of 1:10.

[0068] Comparative Example 2: A method for preparing an anode aluminum foil for an aluminum electrolytic capacitor, comprising the following processes:

[0069] Step (1) pretreatment: place the aluminum foil in a 5% sodium hydroxide solution at 40° C. for 20 seconds;

[0070] Step (2) Pore etching: The aluminum foil obtained after pretreatment is used as the anode and graphite is used as the cathode. Electrolysis is carried out in the porolysis solution at 60°C for 150s with a current density of 0.20A / cm 2 The pore-forming solution includes the following components: 1M hydrochloric acid, 1M sulfuric acid and 0.2M sodium nitrate;

[0071] Step (3) hole expansion corrosion:

[0072] The aluminum foil obtained after pore corrosion was used as the anode and graphite as the cathode. The aluminum foil was electrolyzed in the pore expansion solution at 70°C for 360s with a current density of 0.12A / cm2. The aluminum foil was then washed with 0.25M nitric acid at 30°C and dried at 120°C. The pore expansion solution included the following components: 1M hydrochloric acid and 0.4g / L corrosion inhibitor aniline.

[0073] Step (4) post-processing:

[0074] The aluminum foil obtained after hole expansion corrosion is placed in a boric acid solution for anodization at a voltage of 520V for 20 minutes; it is immersed in a 100% stearic acid solution at 75°C for 20 minutes; and it is dried at 120°C to obtain an anode aluminum foil; the mass concentration of the boric acid solution is 13%, and it contains ammonium pentaborate and boric acid in a mass ratio of 1:10.

[0075] Comparative Example 3: A method for preparing an anode aluminum foil for an aluminum electrolytic capacitor, comprising the following processes:

[0076] Step (1) pretreatment: place the aluminum foil in a 5% sodium hydroxide solution at 40° C. for 20 seconds;

[0077] Step (2) Pore formation corrosion: The aluminum foil obtained after pretreatment is used as the anode and graphite is used as the cathode. Electrolysis is carried out in the porolysis solution at 60°C for 150s with a current density of 0.20A / cm 2 The pore-forming solution includes the following components: 1M hydrochloric acid, 1M sulfuric acid and 0.2M sodium nitrate;

[0078] Step (3) Hole expansion corrosion:

[0079] The aluminum foil obtained after pore corrosion was used as the anode and graphite as the cathode. The aluminum foil was electrolyzed in the pore expansion solution at 70°C for 360s with a current density of 0.12A / cm2. The aluminum foil was then washed with 0.25M nitric acid at 30°C and dried at 120°C. The pore expansion solution included the following components: 1M hydrochloric acid and 0.4g / L corrosion inhibitor polyacrylic acid.

[0080] Step (4) post-processing:

[0081] The aluminum foil obtained after hole expansion corrosion is placed in a boric acid solution for anodization at a voltage of 520V for 20 minutes; it is immersed in a 100% stearic acid solution at 75°C for 20 minutes; and it is dried at 120°C to obtain an anode aluminum foil; the mass concentration of the boric acid solution is 13%, and it contains ammonium pentaborate and boric acid in a mass ratio of 1:10.

[0082] Comparative Example 4: A method for preparing an anode aluminum foil for an aluminum electrolytic capacitor, comprising the following processes:

[0083] Step (1) pretreatment: place the aluminum foil in a 5% sodium hydroxide solution at 40° C. for 20 seconds;

[0084] Step (2) Pore etching: The aluminum foil obtained after pretreatment is used as the anode and graphite is used as the cathode. Electrolysis is carried out in the porolysis solution at 60°C for 150s with a current density of 0.20A / cm 2 The pore-forming solution includes the following components: 1M hydrochloric acid, 1M sulfuric acid and 0.2M sodium nitrate;

[0085] Step (3) hole expansion corrosion:

[0086] The aluminum foil obtained after pore etching was used as the anode and graphite as the cathode. The samples were electrolyzed in a pore expansion solution (1M hydrochloric acid) at 70°C for 360s with a current density of 0.12A / cm2. The samples were then washed with 0.25M nitric acid at 30°C and dried at 120°C.

[0087] Step (4) post-processing:

[0088] The aluminum foil obtained after hole expansion corrosion is placed in a boric acid solution for anodization at a voltage of 520V for 20 minutes; it is immersed in a 100% stearic acid solution at 75°C for 20 minutes; and it is dried at 120°C to obtain an anode aluminum foil; the mass concentration of the boric acid solution is 13%, and it contains ammonium pentaborate and boric acid in a mass ratio of 1:10.

[0089] Experiment: Take the anode aluminum foils obtained in Examples 1-3 and Comparative Examples 1-4 to prepare samples, test their properties and record the test results:

[0090] Specific capacitance test: Use LCR digital bridge to connect the anode aluminum foil, use boric acid solution as the test solution, and detect the specific capacitance of the sample;

[0091] Water resistance test: Use anode foil TV characteristic tester to test the water resistance of the sample. Boil the sample in water and test the time it takes for the voltage to reach 0.9Vf, which is recorded as the boost time.

[0092]

[0093]

[0094] According to the data in the above table, we can clearly draw the following conclusions:

[0095] The anode aluminum foil obtained in Examples 1-3 is compared with the anode aluminum foil obtained in Comparative Examples 1-4. The test results show that:

[0096] Compared with the comparative example, the anode aluminum foil obtained in Examples 1-3 has higher specific capacitance data, and the lower voltage rise time indicates that it has better water resistance, which fully demonstrates that the present invention achieves the improvement of the capacity and performance of the anode aluminum foil for aluminum electrolytic capacitors.

[0097] Compared with Example 1, the slow-release agent used in the hole-expanding corrosion process of Comparative Example 1 is aniline; the pretreatment process of Comparative Example 2 does not contain zinc ions, and the slow-release agent used in the hole-expanding corrosion process is aniline; the pretreatment process of Comparative Example 3 does not contain zinc ions, and the slow-release agent used in the hole-expanding corrosion process is polyacrylic acid; the pretreatment process of Comparative Example 4 does not contain zinc ions, and no slow-release agent is added in the hole-expanding corrosion process. The anode aluminum foil obtained in Comparative Examples 1-4 has deteriorated specific capacitance data and boost time. It can be seen that the setting of the anode aluminum process and the components used in this application can promote the improvement of the capacity and performance of the anode aluminum foil for aluminum electrolytic capacitors.

[0098] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.

[0099] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an anode aluminum foil for an aluminum electrolytic capacitor, characterized in that: Including the following processes: The aluminum foil is sequentially subjected to pretreatment, pore formation corrosion, pore expansion corrosion, and post-treatment to obtain an anode aluminum foil; The pretreatment uses an alkaline solution containing zinc ions to deposit elemental zinc on the surface of the aluminum foil; The hole enlargement etching process is as follows: the aluminum foil obtained after hole etching is used as the anode, and the graphite is used as the cathode. In the hole enlargement solution, at a temperature of 70 to 80° C., electrolysis is performed for 360 to 600 seconds with a current density of 0.08 to 0.12 A / cm 2 ; Then, wash with 0.25-0.30M nitric acid at a temperature of 30-35°C and dry at 120-150°C; The pore-enlarging solution comprises the following components: 1-2M hydrochloric acid, 0.4-1.0g / L corrosion inhibitor; The corrosion inhibitor is an aniline polymer; the aniline polymer is prepared by the following process: In an argon atmosphere, 4-vinylaniline, maleic anhydride, azobisisobutyronitrile and 2-phenyl-2-propylbenzodisulfide are mixed, stirred and reacted at 60-70°C for 12-15 hours to obtain a polymer; rotary evaporation, methanol precipitation, centrifugation and purification; Add deionized water and mix, adjust the pH to 4.0-4.5 with hydrochloric acid, react at 60-70°C for 120-150 minutes with stirring; dry to obtain an aniline polymer; The aniline polymer is prepared from the following molar components: 3-4 parts of 4-vinylaniline, 1-2 parts of maleic anhydride, 6-9 parts of 2-phenyl-2-propylbenzodisulfide, and 0.14-0.21 parts of azobisisobutyronitrile.

2. The method for preparing an anode aluminum foil for an aluminum electrolytic capacitor according to claim 1, characterized in that: The pretreatment process is as follows: placing the aluminum foil in an alkaline solution at 40 to 45° C. for 20 to 60 seconds; The alkaline solution is obtained by dissolving zinc oxide with 5% to 7% sodium hydroxide; the amount of zinc oxide added to the alkaline solution is 0.9 to 1.3 wt%.

3. The method for preparing an anode aluminum foil for an aluminum electrolytic capacitor according to claim 1, characterized in that: The pore etching process is as follows: the aluminum foil obtained after pretreatment is used as an anode, and graphite is used as a cathode. Electrolysis is performed in a pore-forming solution at a temperature of 60 to 80° C. for 90 to 150 seconds, and a current density of 0.15 to 0.20 A / cm 2 ; The pore-forming solution includes the following components: 1M hydrochloric acid, 1-3M sulfuric acid and 0.2-0.3M sodium nitrate.

4. The method for preparing an anode aluminum foil for an aluminum electrolytic capacitor according to claim 1, characterized in that: The post-processing process is as follows: The aluminum foil obtained after hole expansion and corrosion is placed in a boric acid solution for anodization at a voltage of 520 to 720 V for 12 to 20 minutes; The aluminum foil is placed in a stearic acid solution at 75 to 85° C. and immersed in the stearic acid solution at 75 to 85° C. for 20 to 30 minutes; and dried at a temperature of 120 to 150° C. to obtain an anode aluminum foil.

5. The method for preparing an anode aluminum foil for an aluminum electrolytic capacitor according to claim 4, characterized in that: The mass concentration of the boric acid solution is 13% to 17%, and contains ammonium pentaborate and boric acid in a mass ratio of (1 to 3):

10.

6. An anode aluminum foil for aluminum electrolytic capacitors prepared according to the preparation method according to any one of claims 1 to 5.