Lithium ion battery negative electrode active material and preparation method thereof and battery

By using a combination of coated organosiloxane polymer and carbon coating layer in lithium-ion battery anode materials, the problems of insufficient channels and accumulation of side reaction products in traditional inorganic silicon materials are solved, significantly improving the life and performance of the battery.

CN118299550BActive Publication Date: 2024-10-29JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410725514.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-29
Estimated Expiration
2044-06-06

AI Technical Summary

Technical Problem

Inorganic silicon-oxygen (SiOx) materials in traditional lithium-ion battery anode materials have reduced battery life due to insufficient channels and accumulation of side reaction products, and cannot meet the performance needs of new energy vehicles.

Method used

Coated organosiloxane polymer is used as the negative active material of lithium-ion batteries. By forming a carbon coating layer on the surface of silicon-based materials, it broadens the channels of cations, reduces capacitive impedance, and improves structural stability and conductive path gaps.

Benefits of technology

It effectively reduces the expansion rate and deterioration of the battery negative electrode, increases the cycle life, and improves the battery's electrical performance and safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118299550B_ABST
    Figure CN118299550B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of secondary batteries, and in particular to a negative electrode active material for a lithium ion battery, a preparation method thereof, and a battery. A negative electrode active material for a lithium ion battery, comprising: a silicon-based material, and a carbon coating layer coated on the surface of the silicon-based material; wherein the silicon-based material is an organic siloxane polymer, and the organic siloxane polymer comprises a Si-O group and a Si-R group. The preparation method of the negative electrode active material comprises: preparing an organic siloxane polymer, forming a carbon coating layer on the surface of the organic siloxane polymer, and obtaining a negative electrode active material for a lithium ion battery comprising an organic siloxane polymer core and a carbon coating layer shell coated on the outer surface of the organic siloxane polymer. A negative electrode sheet, comprising a negative electrode active material for a lithium ion battery. The present application can alleviate the problem of volume expansion caused by the accumulation of side reaction products on the negative electrode of the battery cell, and the blockage of the conductive network / lack of ion path space, which affects the electrical performance or safety performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary batteries, and in particular to a negative electrode active material for a lithium ion battery, a preparation method thereof, and a battery. Background Art

[0002] In recent years, with the gradual increase in the market share of new energy vehicles, people have also put forward higher requirements for the various performances of new energy vehicles. Electrode materials such as negative electrode materials in secondary batteries have a huge impact on battery performance. Among traditional negative electrode materials, inorganic silicon-oxygen (SiOx) negative electrode materials have major defects. For example, the existing Si-OC channel is not enough for cation intercalation and deintercalation, and other side reaction products do not have time to escape and accumulate on the electrode sheet, which can easily induce rapid deterioration inside the cell, leading to physical expansion of the battery, blockage of the power network, and greatly reducing the battery life and poor cycle stability. This has greatly affected the application of Si elements in battery negative electrode materials.

[0003] In the related art, inorganic silicon materials are mostly used in negative electrode plates containing silicon-based materials. Since it is impossible to increase the silicon content while ensuring energy density and battery life, low-silicon materials are generally used, which makes it impossible for the performance of silicon to be fully exerted in the battery, affecting the electrical performance or safety performance of the battery and failing to meet actual usage requirements. Summary of the invention

[0004] In view of this, the present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the present invention provides a negative electrode active material for a lithium ion battery, a preparation method thereof, and a battery, which can alleviate the problem of volume expansion caused by the accumulation of side reaction products on the negative electrode of the battery cell, blockage of the conductive network / lack of ion path space, and the impact on the electrical performance or safety performance of the battery.

[0005] In order to solve the above technical problems, this application is implemented as follows:

[0006] According to one aspect of the present application, an embodiment of the present application provides a negative electrode active material for a lithium ion battery, the negative electrode active material for a lithium ion battery comprising: a silicon-based material, and a carbon coating layer coated on the surface of the silicon-based material;

[0007] The silicon-based material is an organosiloxane polymer, and the organosiloxane polymer includes a Si-O group and a Si-R group;

[0008] Among them, R is selected from at least one of ethyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, decyl, tert-hexyldimethylchlorosilane, substituted or unsubstituted C6-16 cycloalkyl, substituted or unsubstituted C6-16 aryl, and substituted or unsubstituted C8-16 aralkyl.

[0009] In addition, the lithium-ion battery negative electrode active material according to the present application may also have the following additional technical features:

[0010] In some embodiments, the organosiloxane polymer comprises a group represented by the following formula (I):

[0011]

[0012] Among them, R is selected from at least one of ethyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, decyl, tert-hexyldimethylchlorosilane, substituted or unsubstituted C6-16 cycloalkyl, substituted or unsubstituted C6-16 aryl, and substituted or unsubstituted C8-16 aralkyl; and the value of n is 2 to 10000.

[0013] In some embodiments, the organosiloxane polymer has a planar polygonal network structure. Optionally, the planar polygonal network structure includes a planar tetragonal network structure.

[0014] In some embodiments, the organosiloxane polymer has a cage structure.

[0015] In some embodiments, R is selected from at least one of ethyl, tert-butyl, phenyl or tert-hexyldimethylsilyl chloride.

[0016] In some embodiments, the value of n is 5-8000.

[0017] In some embodiments, the number average molecular weight of the organosiloxane polymer is ≤100,000.

[0018] In some embodiments, the material of the carbon coating layer includes at least one of natural graphite, artificial graphite, soft carbon, hard carbon, graphene, carbon nanotubes, mesophase carbon microbeads or carbon fibers.

[0019] In some embodiments, the carbon coating layer is formed by vapor-phase coating of at least two vapor-phase carbon sources.

[0020] In some embodiments, the gas-phase carbon source includes a first gas-phase carbon source and a second gas-phase carbon source, the first gas-phase carbon source and the second gas-phase carbon source include unsaturated compounds containing alkenyl or alkynyl groups and having no more than 6 carbon atoms, and the first gas-phase carbon source and the second gas-phase carbon source satisfy the following relationship:

[0021] 2≤the unsaturation degree of the first gas-phase carbon source≤the unsaturation degree of the second gas-phase carbon source≤6.

[0022] According to another aspect of the present application, an embodiment of the present application provides a method for preparing a negative electrode active material for a lithium ion battery, the method comprising the following steps:

[0023] preparing a silicon precursor;

[0024] The silicon precursor is used to prepare an organosiloxane polymer, wherein the prepared organosiloxane polymer includes a Si-O group and a Si-R group; wherein R is selected from at least one of ethyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, decyl, tert-hexyldimethylchlorosilane, substituted or unsubstituted C6-16 cycloalkyl, substituted or unsubstituted C6-16 aryl, and substituted or unsubstituted C8-16 aralkyl;

[0025] A carbon coating layer is formed on the surface of the organosiloxane polymer to prepare a lithium ion battery negative electrode active material comprising an organosiloxane polymer core and a carbon coating layer coated on the outer surface of the organosiloxane polymer.

[0026] In some embodiments, the preparation of the silicon precursor specifically includes: uniformly mixing reactants, an organic solvent and a catalyst and reacting them, and removing impurities after the reaction is completed to obtain the silicon precursor;

[0027] The silicon precursor is S(SiHROH)2;

[0028] Alternatively, the silicon precursor is RSi(OH)3 and [RSi(OH)2]2O.

[0029] In some embodiments, the reactants include SiH2ROH and SiH2RSH;

[0030] Alternatively, the reactant comprises RSiCl3.

[0031] In some embodiments, the organic solvent includes at least one of dimethyl sulfoxide, N,N-dimethylformamide, a sulfhydryl-containing compound, an alcohol solvent, or an ether solvent;

[0032] In some embodiments, the catalyst includes at least one of propylene glycol methyl ether acetate, N,N'-dicyclohexylcarbodiimide, aniline or potassium hydroxide.

[0033] In some embodiments, the preparation of the silicon precursor S(SiHROH)2 specifically includes: mixing the first reactant, the second reactant and the organic solvent evenly, and then adding the catalyst and the auxiliary agent and mixing evenly to obtain a mixed solution; reacting the mixed solution under the conditions of a first temperature and ultraviolet light irradiation, and obtaining an oily solution after the reaction; and successively warming and heating the oily solution in an inert gas atmosphere to obtain the silicon precursor;

[0034] The first reactant is a compound comprising a silylene group, a hydroxyl group and an R group, and the second reactant is a compound comprising a silylene group, a sulfhydryl group and an R group; the R group is selected from at least one of ethyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, decyl, substituted or unsubstituted C6-16 cycloalkyl, substituted or unsubstituted C6-16 aryl, and substituted or unsubstituted C8-16 aralkyl.

[0035] In some embodiments, the chemical formula of the first reactant is SiH2ROH; the chemical formula of the second reactant is SiH2RSH.

[0036] In some embodiments, the auxiliary agent includes formic acid.

[0037] In some embodiments, the molar ratio of the sum of the amounts of the first reactant and the second reactant to the auxiliary agent, the organic solvent and the catalyst is (2-8): (0.8-6): (22-30): (0.04-0.5); wherein the molar ratio of the first reactant to the second reactant is 1: (1-1.5).

[0038] In some embodiments, the first temperature is -2°C to 5°C, and the ultraviolet lamp irradiation reaction time is 30min to 60min; and / or the rewarming temperature is 20°C to 30°C; and / or the heating temperature is 100°C to 150°C, and the heating time is 1h to 3h.

[0039] In some embodiments, the preparation of the silicon precursor RSi(OH)3 includes: uniformly mixing the reactants, organic solvent and catalyst, reacting at a temperature ≤30°C, filtering and distilling after the reaction to obtain the silicon precursor RSi(OH)3.

[0040] In some embodiments, the preparation of the silicon precursor [RSi(OH)2]2O includes: uniformly mixing reactants, an organic solvent, a catalyst and Si2O, reacting at a temperature ≤30°C, filtering and distilling after the reaction to obtain the silicon precursor [RSi(OH)2]2O.

[0041] The reactant includes RSiCl3. The molar ratio of the reactant, the solvent and the catalyst is (4-8): (15-30): (0.5-2).

[0042] In some embodiments, the preparation of the organosiloxane polymer specifically includes:

[0043] The silicon precursor, the organic solvent and the catalyst are mixed uniformly, and the temperature and pressure are increased to the second temperature and the first pressure in an inert gas atmosphere to react, and after the reaction is completed, the temperature and pressure are decreased to the third temperature and the second pressure in an inert gas atmosphere, and separated to obtain the organosiloxane polymer. Wherein, the second temperature is 120°C to 180°C, and the first pressure is 1.0atm to 3.0atm; and / or, the reaction time at the second temperature and the first pressure is 70h to 100h; and / or, the third temperature is 22°C to 28°C, and the second pressure is 0.9atm to 1.1atm.

[0044] In some embodiments, the molar ratio of the silicon precursor, the organic solvent and the catalyst is 1:(12-20):(0.4-0.85).

[0045] In some embodiments, the temperature increase rate is 1-5° C. / h, and the pressure increase rate is 0.04-0.08 atm / h.

[0046] In some embodiments, the temperature reduction rate is 0.5-5°C / h, and the pressure reduction rate is 0.02-0.08atm / h.

[0047] In some embodiments, the inert gas includes at least one of argon, helium, or neon.

[0048] In some embodiments, the organosiloxane polymer is used as a matrix material, and an atomic layer deposition process is used to form a carbon coating layer on the surface of the organosiloxane polymer.

[0049] In some embodiments, forming a carbon coating layer on the surface of the organosiloxane polymer specifically includes:

[0050] Introducing a carrier gas into an atomic layer deposition device, placing an organosiloxane polymer into the atomic layer deposition device, introducing a first gas-phase carbon source, and performing a first gas-phase deposition after heating to perform a first stage of carbon coating on the surface of the organosiloxane polymer;

[0051] The temperature is then lowered, and a second gas-phase carbon source is introduced. After the temperature is raised, a second gas-phase deposition is performed to perform a second stage of carbon coating on the surface of the organic siloxane polymer, and a carbon coating layer is formed on the surface of the organic siloxane polymer to obtain a lithium ion battery negative electrode active material including an organic siloxane polymer and a carbon coating layer.

[0052] In some embodiments, the heating temperature is 20° C. to 40° C., and the heating time is 2 h to 5 h.

[0053] In some embodiments, the cooling temperature is ≤20°C, and the cooling time is 3h to 6h.

[0054] In some embodiments, the first gas-phase carbon source and the second gas-phase carbon source satisfy the following relationship:

[0055] 2≤the unsaturation degree of the first gas-phase carbon source≤the unsaturation degree of the second gas-phase carbon source≤6.

[0056] In some embodiments, taking the amount of the organosiloxane polymer as 1 eq as a reference, the gas flow rates of the first gas-phase carbon source and the second gas-phase carbon source satisfy the following relationship:

[0057] 1eq≤the gas flow rate of the first gas-phase carbon source≤the gas flow rate of the second gas-phase carbon source≤4eq.

[0058] According to another aspect of the present application, an embodiment of the present application provides a negative electrode plate, which includes the aforementioned lithium ion battery negative electrode active material or the lithium ion battery negative electrode active material prepared according to the aforementioned method.

[0059] According to another aspect of the present application, an embodiment of the present application provides a battery, which includes the negative electrode plate described above.

[0060] As an extension of the concept of the present invention, an electrical device is also provided, and the electrical device includes the battery.

[0061] Implementing the technical solution of the present invention has at least the following beneficial effects:

[0062] In the embodiment of the present application, the negative electrode active material of the lithium ion battery and the preparation method thereof are a new type of negative electrode active material and the preparation method thereof that can be applied to batteries such as lithium ion secondary batteries. The negative electrode active material of the lithium ion battery is an organic-inorganic composite material formed by coating a silicon-based material, especially an organic silicon material, with a carbon material. The negative electrode active material of the lithium ion battery breaks the spatial limitation of the traditional inorganic silicon (mainly SiOx) by introducing a new silicon-based material, namely an organic siloxane polymer, so that the channel of the cation can be greatly widened in space, and the capacitance impedance is reduced. At the same time, the structure of the organic siloxane polymer increases its intercalation freedom for the cation, which has a positive effect on the problem of cation deintercalation on the negative electrode.

[0063] Compared with the existing inorganic silicon SiOx materials, the provided lithium-ion battery negative electrode active material of the organosiloxane polymer containing Si-O groups and Si-R groups has good structural stability and large gaps in the conductive path, which can reduce the probability of side reactions and improve the retention of side reaction products on the electrode sheet. This can reduce the expansion rate of the negative electrode sheet of the battery or reduce the degradation of the negative electrode of the battery, that is, it can improve the accumulation of side reaction products on the negative electrode of the battery cell, resulting in volume expansion, conductive network blockage / insufficient ion path space, which can affect the electrical performance or safety performance of the battery, thereby helping to improve the cycle life of the battery.

[0064] Additional aspects and advantages of the present application will be given in part in the following description, and in part will become obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] The above and other purposes, features and advantages of the present invention will become more apparent by describing the embodiments of the present invention in more detail in conjunction with the accompanying drawings. The accompanying drawings are used to provide a further understanding of the embodiments of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention.

[0066] Figure 1 Shown is a spatial model diagram (planar polygonal network structure) of an organosiloxane polymer provided by an embodiment of the present invention.

[0067] Figure 2 Shown is a spatial model diagram (cage-type structure) of another organosiloxane polymer provided in an embodiment of the present invention.

[0068] Figure 3 Shown is an NMR (nuclear magnetic resonance) graph (frequency 400 Hz, deuterated reagents DMSO, CDCl3) of a reactant (SiH2ROH) provided in an embodiment of the present invention.

[0069] Figure 4 Shown is the NMR graph (frequency 400 Hz, deuterated reagents DMSO, CDCl3) of another reactant (SiH2RSH) provided in an embodiment of the present invention.

[0070] Figure 5 Shown is the NMR graph-C spectrum (frequency 400 Hz, deuterated reagent CDCl3) of another reactant (RSiCl3) provided in an embodiment of the present invention.

[0071] Figure 6 Shown is the NMR spectrum of another reactant (RSiCl3) provided in an embodiment of the present invention -H spectrum (frequency 400 Hz, deuterated reagent CDCl3).

[0072] Figures 3 to 6 In the above, PPM represents chemical shift value. DMSO is dimethyl sulfoxide, and CDCl3 is deuterated chloroform. DETAILED DESCRIPTION

[0073] The present application is further described below in conjunction with specific embodiments. It should be understood that these embodiments of the present application are only used to illustrate the present application and are not used to limit the scope of the present application.

[0074] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range or the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0075] In the related art, the silicon-based materials in the negative electrode active materials of lithium-ion batteries are mostly inorganic silicon (SiO x ) materials, however, in the existing pole pieces containing inorganic Si (silicon), since it is impossible to increase the silicon content while ensuring energy density and battery life, low-silicon materials are generally used, which makes it impossible for the performance of silicon to be fully exerted in the battery. Compared with inorganic silicon, as a member of high-performance materials, the spatial structural characteristics of organic silicon directly expand the ion transmission channel. Such a spatial scale of the transmission path greatly improves the free embedding / combination of ions and the detachment of pole piece deposits. Therefore, the use of organic silicon materials as lithium-ion battery negative electrode active materials is extremely beneficial to the long-term reliability and safety of power batteries.

[0076] In view of this, the present application proposes a novel organosilicon material and a preparation method thereof, and applies the organosilicon material to the negative electrode active material of lithium-ion batteries, providing a negative electrode active material that can be used in secondary batteries such as lithium-ion batteries or sodium-ion batteries, which can be used to improve the volume expansion caused by the accumulation of side reaction products on the negative electrode of the battery cell, the blockage of the conductive network / the lack of ion path space, and the impact on the electrical performance or safety performance of the battery. The specific technical solution is described below.

[0077] 1. Lithium-ion battery negative electrode active material and preparation method thereof

[0078] In some embodiments, the present application provides a negative electrode active material for a lithium ion battery, which includes: a silicon-based material, and a carbon coating layer coated on the surface of the silicon-based material.

[0079] The negative electrode active material of the lithium ion battery includes a silicon-based material and a carbon coating layer coated on the surface of the silicon-based material, that is, the negative electrode active material of the lithium ion battery can be a core-shell structure, the core layer (core) is a silicon-based material, the shell layer (shell) is a carbon coating layer, and the carbon coating layer is coated on at least part of the outer surface of the silicon-based material. The carbon coating layer is mainly formed by carbon material, that is, it mainly contains carbon elements. In addition, other elements can be introduced into the carbon coating layer to facilitate its function, which is not limited in this embodiment.

[0080] It should be noted that in the present application, the "coating" is not limited to direct coating, but also includes indirect coating. For example, the coating layer coats the silicon-based material, and there may be no other structure between the coating layer and the outer surface of the silicon-based material, or there may be one or more layers of other structures between the coating layer and the outer surface of the silicon-based material. Preferably, there is no other structure between the coating layer and the outer surface of the silicon-based material.

[0081] The coating layer is formed or coated on at least part of the surface of the silicon-based material, which can protect the silicon-based material and improve the structural stability of the negative electrode active material of the lithium-ion battery. The coating layer is formed or coated on at least part of the surface of the silicon-based material means that the coating layer can completely encapsulate the silicon-based material in the coating layer, or the coating layer can only coat part of the outer surface of the silicon-based material; that is, the coating layer can completely coat the silicon-based material, or it can coat part of the surface of the silicon-based material, preferably completely coating.

[0082] In the present application, the silicon-based material is an organosiloxane polymer, which includes a Si-O group and a Si-R group; wherein R is selected from at least one of ethyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, decyl, tert-hexyldimethylchlorosilane, substituted or unsubstituted C6-16 cycloalkyl, substituted or unsubstituted C6-16 aryl, and substituted or unsubstituted C8-16 aralkyl.

[0083] The provided lithium-ion battery negative electrode active material is mainly composed of carbon materials such as traditional carbon materials (composite graphite, biomass-based hard carbon / soft carbon, gas-phase carbon source, etc.) coated with organic siloxane polymers. The lithium-ion battery negative electrode active material can greatly widen the channel of cations in space and reduce the capacitance impedance by introducing a new type of organic siloxane polymer. At the same time, its structure increases its intercalation freedom for cations, which has a positive effect on the problem of cation deintercalation on the negative electrode.

[0084] The structure of the negative electrode active material of the lithium ion battery can be a spatial cubic coating structure. The design unit of the negative electrode active material of the lithium ion battery is centered on the organic-inorganic composite material, and the coating of the negative electrode active material of the lithium ion battery is a specific implementation mode to form a material unit of a new negative electrode space structure.

[0085] The lithium-ion battery negative electrode active material of the present application can break the spatial limitations of traditional inorganic silicon (mainly SiOx) by adopting an organic siloxane polymer silicon-based material. The provided organic siloxane polymer material is a cubic hole structure. The organic silicon material has advantages from reaction synthesis to the interlayer structure compared with traditional carbon materials such as graphite. In addition, by adopting the organic siloxane polymer material, it can also form a coating structure with many negative electrode carbon materials such as graphite, soft and hard carbon, carbon nanotubes, etc. Compared with the power battery using traditional inorganic silicon materials as the negative electrode active material, the power battery including the negative electrode active material of the organic-inorganic composite material provided in the embodiment of the present application has a greatly enhanced advantage in the spatial electrical signal transmission performance.

[0086] In some embodiments, the organosiloxane polymer comprises a group as shown in the following formula (I), or the structure of the organosiloxane polymer is as shown in formula (I):

[0087]

[0088] Among them, R is selected from at least one of ethyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, decyl, tert-hexyldimethylchlorosilane, substituted or unsubstituted C6-16 cycloalkyl, substituted or unsubstituted C6-16 aryl, and substituted or unsubstituted C8-16 aralkyl; and the value of n is 2 to 10000.

[0089] In the embodiment of the present application, in the formula I of the organosiloxane polymer, R can be ethyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, decyl, tert-hexyldimethylchlorosilane, substituted or unsubstituted C6-16 cycloalkyl, substituted or unsubstituted C6-16 aryl, substituted or unsubstituted C8-16 arylalkyl, etc. The R group is preferably a group containing an even number of carbon atoms, such as ethyl, butyl, cycloalkyl containing an even number of carbon atoms, aryl containing an even number of carbon atoms, etc.

[0090] The term "aryl" refers to a closed aromatic ring or ring system. For example, aryl can be a C6-C16 aryl, a C6-C12 aryl, a C6-C10 aryl, a C6-C8 aryl, wherein the C6-C16 aryl refers to a carbon atom containing 6-16 for forming a ring. In certain embodiments, aryl includes phenyl, naphthyl, phenanthrenyl, anthryl, biphenyl, triphenylene, pyrenyl, etc. In addition, aryl can be optionally substituted. In the present embodiment, aryl is preferably an aryl comprising an even number of carbon atoms.

[0091] The term "cycloalkyl" encompasses cyclic alkyl groups. Cycloalkyl groups may be C6-16 cycloalkyl groups (cycloalkyl groups of 6 to 16 carbon atoms), C6-12 cycloalkyl groups, C6-10 cycloalkyl groups, C6-8 cycloalkyl groups, C6-12 cycloalkyl groups, etc. For example, cycloalkyl groups may be cyclohexyl groups, cyclooctyl groups, etc. In addition, cycloalkyl groups may be optionally substituted. In the present embodiment, cycloalkyl groups are preferably cycloalkyl groups containing an even number of carbon atoms.

[0092] Similarly, the term "aralkyl" and the like have the meaning commonly understood in the art and will not be described in detail herein.

[0093] Unless otherwise specified, the compounds or functional groups used herein may be substituted or unsubstituted. The term "substituted" used herein means that at least one hydrogen atom contained in the compound or functional group is replaced by at least one substituent selected from the following groups: C2-C10 alkyl and derivatives thereof, C2-C10 alkoxy and derivatives thereof, C2-C10 aralkyl and derivatives thereof, etc.

[0094] As an improvement of the negative electrode active material of the lithium ion battery of the present application, R can be selected from any one of ethyl, isobutyl, sec-butyl, tert-butyl, tert-hexyldimethylchlorosilane, substituted or unsubstituted C6-16 aryl; preferably, the aryl is selected from phenyl. More preferably, R is selected from at least one of tert-hexyldimethylchlorosilane, ethyl, tert-butyl or phenyl.

[0095] The provided organosiloxane polymer can increase the physical and chemical stability of the generated organosiloxane polymer, especially improve the physical properties of the material, and have better physical stability, by rationally planning the side chain R group, especially by using an alkyl group, an aryl group or an arylalkyl group containing an even number of carbon atoms, more preferably using tert-hexyldimethylchlorosilane, ethyl, tert-butyl or phenyl.

[0096] In the embodiment of the present application, in the general formula I of the organosiloxane polymer, the value of n is 2 to 10000. Further, the value of n can be 5 to 8000. Further, the value of n can be 1000 to 7000. By controlling the value of n within a reasonable range, the molecular weight of the prepared organosiloxane polymer can be within a suitable range, which is beneficial to improving the stability of the organosilicon material.

[0097] In some embodiments, the number average molecular weight of the organosiloxane polymer is ≤100,000. Further, the number average molecular weight of the organosiloxane polymer is ≤80,000. Further, the number average molecular weight of the organosiloxane polymer is ≤70,000. There is no specific limit on the lower limit of the number average molecular weight of the organosiloxane polymer. In addition, the specific value of the number average molecular weight of the organosiloxane polymer can be selected and regulated according to actual conditions and is not limited here.

[0098] By making the number average molecular weight of the organosiloxane polymer within the above range, the bonding strength between the organosiloxane polymer and the carbon material is relatively strong. During the long-term cycle of the secondary battery, the coating layer is not easy to fall off from the surface of the organosilicone material, which is beneficial to ensure the cycle performance of the secondary battery.

[0099] In some embodiments, the organosiloxane polymer has a planar polygonal mesh structure; optionally, the planar polygonal mesh structure includes a planar tetragonal mesh structure. It should be noted that the organosiloxane polymer provided in the embodiment of the present application has a spatial three-dimensional mesh structure as a whole, and the three-dimensional mesh structure is a three-dimensional mesh structure formed by interconnecting multiple layers of planar polygonal structures; for example, multiple levels (multi-layer planar polygonal structures) can be linked together by series-parallel connection between Si-O skeletons and R groups. Exemplarily, the above-mentioned planar polygonal mesh structure may include but is not limited to a planar tetragonal mesh structure, a planar hexagonal mesh structure or other planar regular or irregular mesh structures, etc., which are not limited in this embodiment. For simplicity, the following mainly takes the organosiloxane polymer with a planar tetragonal mesh structure as an example for explanation.

[0100] In other embodiments, the organosiloxane polymer has a cage structure.

[0101] In the present application, the spatial model of the organosiloxane polymer can have a variety of structural forms. For example, in some cases, it can be a planar tetragonal lattice network structure; however, the spatial model of the organosiloxane polymer is not limited to this. For example, the organosiloxane polymer can also have a cage structure.

[0102] The above-mentioned organosiloxane polymer structure is mainly based on Si-O and Si-R bonding; in the structure of the organosiloxane, the spatial structure of the ion channel is very open, and ions of the size of Pd (palladium) cations can pass through. The larger the conductive channel space, the better the conductive performance can be. Thus, in some cases, the organosiloxane polymer provided by the present application can have a planar tetragonal lattice mesh structure, and its spatial model is more three-dimensional, the gap of the conductive path is larger, and the physical stability is better than that of the existing inorganic silicon materials. By controlling the side chain R linked to the Si element in the polymer monomer, the physical properties attached to the organosilicon material can be controlled. Alternatively, in other cases, the organosiloxane polymer provided by the present application can have a cage structure, and the spatial model of this structure is more three-dimensional, the gap of the conductive path is larger, and the physical stability is better than that of the existing inorganic silicon materials. By controlling the side chain R of the Si element on the 8 corners, the physical properties attached to the organosilicon material can be controlled.

[0103] As an example, Figure 1 shows a spatial model diagram of an organosiloxane polymer provided by some embodiments of the present application, Figure 2 The spatial model diagram of the organosiloxane polymer provided in some other embodiments of the present application is shown. Figure 1 As shown, the provided organosiloxane polymer has a planar polygonal mesh structure (such as a planar tetragonal mesh structure) spatial model. Compared with existing inorganic silicon materials, the planar polygonal mesh structure has a more three-dimensional spatial model, a larger gap in the conductive path, and better physical stability. By controlling the side chain R linked to the Si element in the polymer monomer, the physical properties attached to the organosilicon material can be regulated.

[0104] like Figure 2 As shown, the provided organosiloxane polymer has a cage-type structure space model. Compared with the existing inorganic silicon materials, the cage-type structure space model is more three-dimensional, the gap of the conductive path is larger, and the physical stability is better. By controlling the side chain R of the Si element at the 8 corners, the physical properties attached to the organosilicon material can be controlled.

[0105] Therefore, by using the organosiloxane polymer of the embodiment of the present application and rationally planning the connected side chain R group, the physical and chemical stability of the generated organosiloxane polymer can be increased. Furthermore, the coated negative electrode active material containing the organosiloxane polymer is applied to the battery. In the reaction inside the battery, the coating of the organosilicon material will reduce the occurrence of side reactions due to its chemical properties that are difficult to react; even if some side reactions occur, the generation rate of the side reaction products will be greatly reduced. Alternatively, if the generation rate of the side reaction products is slow and sufficient to slowly detach from the gaps in the spatial structure of the material, the expansion and degradation of the battery will also be greatly improved.

[0106] Based on the above analysis, it can be known that the negative electrode active material of the lithium-ion battery, by adopting the above-mentioned organic siloxane polymer with a planar tetragonal lattice network structure or a cage structure, has a larger conductive channel and better stability, which can reduce the occurrence of side reactions, and thus can improve the accumulation of side reaction products on the negative electrode of the battery cell, resulting in volume expansion, conductive network blockage / inadequate ion path space, which can affect the electrical performance or safety performance of the battery.

[0107] In some embodiments, the material of the carbon coating layer includes, but is not limited to, any one or more combinations of natural graphite, artificial graphite, soft carbon, hard carbon, graphene, carbon nanotubes, mesophase carbon microspheres or carbon fibers. Optionally, in some embodiments, the material of the carbon coating layer includes a group consisting of natural graphite, artificial graphite, soft carbon, hard carbon and a combination thereof. Alternatively, in some embodiments, the carbon coating layer can be formed by gas-phase coating of at least two gas-phase carbon sources, such as by depositing a gas-phase carbon source, especially two or more gas-phase carbon sources, on the surface of the organosilicon material to form a carbon coating layer.

[0108] In the provided lithium-ion battery negative electrode active material, the carbon coating layer can adopt traditional carbon materials, such as graphite, soft carbon, hard carbon, carbon nanotubes and other carbon materials. These traditional carbon materials are widely available, easy to obtain, and meet the use requirements.

[0109] In some embodiments, the gas-phase carbon source includes a first gas-phase carbon source and a second gas-phase carbon source, the first gas-phase carbon source and the second gas-phase carbon source include unsaturated compounds containing alkenyl or alkynyl groups and having no more than 6 carbon atoms, and the first gas-phase carbon source and the second gas-phase carbon source satisfy the following relationship:

[0110] 2≤the unsaturation degree of the first gas-phase carbon source≤the unsaturation degree of the second gas-phase carbon source≤6.

[0111] Optionally, the first gas-phase carbon source may be selected from acetylene, propyne, butyne and the like; or, the first gas-phase carbon source may be a mixture of acetylene and other acetylenic substances and carbon monoxide.

[0112] Optionally, the second gas-phase carbon source can be selected from furan and the like.

[0113] In this way, by using the above two gas-phase carbon sources for coating, the coated material layer can be made smoother and more precise, that is, the formed coating layer can be easier to control, the coating layer thickness can be more uniform, and the protective performance for the active components can be uniform.

[0114] Based on the same inventive concept, in some embodiments, a method for preparing a negative electrode active material for a lithium ion battery is provided, the method comprising the following steps:

[0115] preparing a silicon precursor;

[0116] The organic siloxane polymer is prepared by using a silicon precursor, and the prepared organic siloxane polymer includes a Si-O group and a Si-R group; wherein R is selected from at least one of ethyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, decyl, tert-hexyldimethylchlorosilane, substituted or unsubstituted C6-16 cycloalkyl, substituted or unsubstituted C6-16 aryl, and substituted or unsubstituted C8-16 aralkyl;

[0117] A carbon coating layer is formed on the surface of the organic siloxane polymer to prepare a lithium ion battery negative electrode active material including an organic siloxane polymer core and a carbon coating layer coated on the outer surface of the organic siloxane polymer.

[0118] In this embodiment, when preparing the negative electrode active material of the lithium ion battery, the organosiloxane polymer is first prepared, and then carbon coating is performed on the surface of the organosiloxane polymer to form a carbon coating layer on the surface of the organosiloxane polymer to obtain the negative electrode active material of the lithium ion battery.

[0119] It should be understood that the selection of the organosiloxane polymer, carbon coating layer material, etc. in the preparation method of the negative electrode active material of the lithium ion battery of the present application is the same as the definition made in the negative electrode active material of the lithium ion battery mentioned above in the present application. Please refer to the description of the negative electrode active material of the lithium ion battery mentioned above, and no further details will be given here.

[0120] The preparation method of the negative electrode active material of the lithium ion battery is simple in process, highly feasible, under relatively mild conditions, easy to operate, and suitable for industrial-scale production. In particular, the synthesis and preparation method of the organosiloxane polymer in the negative electrode active material of the lithium ion battery is simple, the environment is easy to control manually, and the toxicity is less, the risk factor is low, and it can provide convenience for mass production. The synthesis and preparation of the organosiloxane polymer will be described in detail below.

[0121] In some embodiments, the preparation of the organosiloxane polymer includes: first preparing a silicon precursor, and then using the silicon precursor to prepare the organosiloxane polymer; wherein the preparation of the silicon precursor specifically includes:

[0122] The reactants, organic solvent and catalyst are mixed evenly and reacted, and after the reaction is completed, impurities are removed to obtain a silicon precursor.

[0123] Optionally, in some cases, the silicon precursor is S(SiHROH)2; the above reactants include SiH2ROH and SiH2RSH. Thus, the silicon precursor can be used to prepare an organosiloxane polymer having a planar polygonal network structure such as a planar tetragonal network structure.

[0124] Alternatively, in some cases, the silicon precursor is RSi(OH)3 and [RSi(OH )2 ]2O; the above-mentioned reactant includes RSiCl3. Thus, the silicon precursor can be used to prepare an organosiloxane polymer having a cage structure.

[0125] The following describes in detail the preparation methods of the organosiloxane polymer having a planar polygonal network structure such as a planar tetragonal network structure and the preparation methods of the organosiloxane polymer having a cage structure.

[0126] In some embodiments, the preparation of an organosiloxane polymer having a planar tetragonal lattice network structure specifically comprises:

[0127] The first reactant, the second reactant and the organic solvent are mixed evenly, and then a catalyst and an auxiliary agent are added and mixed evenly to obtain a mixed solution;

[0128] The mixed solution is reacted at a first temperature (preferably a low temperature environment) and irradiated with an ultraviolet lamp, and an oily solution is obtained after the reaction is completed;

[0129] The oily solution is successively warmed up and heated in an inert gas atmosphere to obtain a silicon precursor;

[0130] The silicon precursor, the organic solvent and the catalyst are uniformly mixed, and the temperature and pressure are increased to a second temperature and a first pressure in an inert gas atmosphere to react. After the reaction is completed, the temperature and pressure are decreased to a third temperature and a second pressure in an inert gas atmosphere, and separated to obtain an organosiloxane polymer;

[0131] Among them, the first reactant is a compound containing a silylene group (SiH2-), a hydroxyl group (-OH) and an R group, and the second reactant is a compound containing a silylene group (SiH2-), a sulfhydryl group (-SH) and an R group; the R group is selected from at least one of ethyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, decyl, substituted or unsubstituted C6-16 cycloalkyl, substituted or unsubstituted C6-16 aryl, and substituted or unsubstituted C8-16 aralkyl.

[0132] The reaction mechanism of the synthesis and preparation of the organosiloxane polymer is that the -SH group is subjected to ultraviolet (UV) irradiation in a low temperature environment, and the -SH group undergoes dehydrogenation and condensation reaction to generate a silicon precursor. Specifically, under the conditions of a catalyst and ultraviolet irradiation, the -SH group is converted from hydrogen to S· in a low temperature environment (such as around 0°C), and at the same time, the Si-H bond of the reactant with the -SH group, i.e., the second reactant, is broken and dehydrogenated; then S· combines with Si on another raw material, i.e., the first reactant, to form a silicon precursor.

[0133] After the silicon precursor synthesis reaction is completed, the silicon precursor can be purified by heating in an inert atmosphere such as a rare gas atmosphere for a period of time to remove impurities (turn off UV irradiation at this time) to obtain a silicon precursor.

[0134] Furthermore, after obtaining the silicon precursor solution, a reaction of preparing an organic siloxane polymer material from the silicon precursor is carried out. The silicon precursor generated and purified by the above reaction is subjected to a condensation reaction to remove H2S & H2O (hydrogen sulfide and water) in an inert atmosphere such as a rare gas atmosphere and a second temperature (high temperature) environment. The S-Si bond and Si-H bond of the silicon precursor are broken, and in a rare gas environment, the above-generated material is heated and pressurized (such as a temperature in the range of 120 to 180°C and an air pressure in the range of 1 to 3 atm), and then, under the catalysis of a catalyst, the silicon precursor undergoes the above-mentioned self-polymerization reaction to generate a high polymer silane, that is, an organic siloxane polymer is obtained.

[0135] In some specific embodiments, the method for preparing the organosiloxane polymer comprises the following steps:

[0136] S100, preparing a silicon precursor, specifically comprising:

[0137] S110, uniformly mixing the first reactant, the second reactant and the organic solvent, then adding the catalyst and the auxiliary agent and mixing them uniformly to obtain a mixed solution; reacting the mixed solution under the conditions of a first temperature (low temperature environment) and irradiation with an ultraviolet lamp, and obtaining an oily solution after the reaction is completed.

[0138] S120, successively warming and heating the oily solution in an inert gas (such as a rare gas) atmosphere to obtain a silicon precursor.

[0139] Optionally, the first reactant is a compound comprising a silylene group, a hydroxyl group and an R group, and illustratively, the chemical formula of the first reactant is SiH2ROH. Optionally, the second reactant is a compound comprising a silylene group, a sulfhydryl group and an R group, and illustratively, the chemical formula of the second reactant is SiH2RSH. Wherein, R can be an ethyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a hexyl group, an octyl group, a decyl group, a substituted or unsubstituted C6-16 cycloalkyl group, a substituted or unsubstituted C6-16 aryl group, a substituted or unsubstituted C8-16 aralkyl group, etc. Preferably, R is selected from at least one of an ethyl group, a tert-butyl group or a phenyl group.

[0140] Optionally, the organic solvent includes, but is not limited to, at least one of dimethyl sulfoxide (DMSO), dimethylformamide (DMF), a thiol-containing compound or an alcohol solvent; for example, the organic solvent may be DMSO, may be DMF, may be a thiol-containing compound, or may be an alcohol solvent, etc. Preferably, the organic solvent is selected from DMSO or DMF, which can reduce side reactions and has good stability. Of course, in other embodiments, the organic solvent is not limited thereto, and an alcohol solvent such as an easily soluble -SH, an organic solvent with low side reactions and good stability can be applied to the present reaction.

[0141] Optionally, the catalyst includes, but is not limited to, at least one of propylene glycol methyl ether acetate (PGMEA) or N,N'-dicyclohexylcarbodiimide (DCC); for example, the catalyst may be PGMEA, or DCC, or a mixture of the two.

[0142] Optionally, the auxiliary agent includes, but is not limited to, formic acid. By adding auxiliary agents such as formic acid, the side reactions can be reduced and the reaction yield can be improved.

[0143] In addition, in other embodiments, organic solvents, catalysts, additives, etc. are not limited to the ones listed above. Under the condition of meeting the requirements of low side reactions and not affecting the performance of the prepared organosiloxane polymer, organic solvents, catalysts, additives, etc. can also be of other types, which will not be described in detail one by one here.

[0144] Optionally, the molar ratio of the sum of the amounts of the first reactant and the second reactant to the auxiliary agent, organic solvent and catalyst is (2-8): (0.8-6): (22-30): (0.04-0.5). Further, the molar ratio of the sum of the amounts of the first reactant and the second reactant to the auxiliary agent, organic solvent and catalyst is (3-7): (1-5): (23-28): (0.08-0.3). For example, the molar ratio of the sum of the amounts of the first reactant and the second reactant to the auxiliary agent, organic solvent and catalyst can be 2: 0.8: 22: 0.04, 2: 1: 25: 0.08, 5: 1: 23: 0.15, 6: 2: 23: 0.3, 7: 4: 23: 0.42, 8: 5.5: 28: 0.4, 8: 6: 30: 0.5, etc.

[0145] The addition amount of the above substances can be adjusted according to the specific usage and the specific reaction progress to optimize the addition amount, reduce side reactions, increase yield and reduce costs.

[0146] The molar ratio of the first reactant to the second reactant is 1:(1-1.5). Furthermore, the molar ratio of the first reactant to the second reactant is 1:(1-1.2). The molar ratio of the first reactant to the second reactant can be close to 1:1, but based on the synthesis reaction mechanism of the silicon precursor, the second reactant containing the -SH group can be added slightly more. For example, the molar ratio of the first reactant to the second reactant can be 1:1.05, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, etc.

[0147] Optionally, the inert gas includes, but is not limited to, at least one of argon, helium or neon. The inert gas may be a rare gas, such as argon, helium, neon and other rare gases. Of course, in other embodiments, other types of inert gases may also be used, as long as they do not limit the purpose of this application, and they are not listed here one by one.

[0148] Optionally, the first temperature is a low temperature, and the first temperature can be set at about 0°C, for example, the first temperature can be -2°C to 5°C, further, the first temperature can be -1°C to 3°C; the first temperature can be, for example, -2°C, -1°C, 0°C, 1°C, 2°C, 3°C, 4°C, 5°C, etc. Optionally, the ultraviolet light irradiation reaction time is 30min to 60min; further, the ultraviolet light irradiation reaction time is 40min to 50min; the ultraviolet light irradiation reaction time can be, for example, 30min, 40min, 50min, 60min, etc.

[0149] Optionally, the temperature of the warming-up can be room temperature, such as room temperature can be about 25°C, for example, the temperature of the warming-up can be 20°C to 30°C; further, the temperature of the warming-up can be 24°C to 26°C. Optionally, the heating temperature is 100°C to 150°C, and the heating time is 1h to 3h. Further, the heating temperature is 120°C to 130°C, and the heating time is 1.5h to 2h. The purpose of warming up and heating the oily liquid is to remove excess solvents, newly generated volatile impurities and other gaseous impurities. That is, under the conditions of the above-mentioned warming-up temperature and heating temperature, the silicon precursor can be effectively removed and purified.

[0150] In step S100, by subjecting the sulfhydryl group (-SH) to ultraviolet (UV) irradiation in a low temperature environment, the -SH group undergoes dehydrogenation and condensation reaction to generate a silicon precursor. Specifically, under the conditions of a catalyst and ultraviolet irradiation, the -SH group is converted from hydrogen to S· in a low temperature environment (such as around 0°C), and at the same time, the Si-H bond of the reactant with the -SH group, i.e., the second reactant, is broken and dehydrogenated; then S· combines with the Si on another raw material, i.e., the first reactant, to form a silicon precursor. And, after the reaction is completed, the temperature is raised for a period of time in a rare gas atmosphere to remove impurities and purify the generated silicon precursor (turn off the UV irradiation at this time).

[0151] Exemplarily, the step of preparing a silicon precursor in S100 specifically includes:

[0152] According to the ratio, the first reactant SiH2ROH, the second reactant SiH2RSH and the organic solvent are added to the flask and mixed, and stirred for 2 to 5 minutes until the mixture is uniform; after stirring and mixing uniformly, the catalyst and the auxiliary agent are added according to the ratio at room temperature, and then a large container is placed outside the flask, and a large amount of crushed ice and water mixture is added to the large container (do not drop it into the flask, and leave a UV lamp irradiation hole / surface) so that the ambient temperature is maintained at the first temperature, that is, maintained at about 0°C; then, the mixture in the flask is irradiated with ultraviolet light through the reserved UV irradiation hole / surface, and the reaction begins. After a period of reaction, such as 30 minutes to 60 minutes, the reaction ends, the ultraviolet lamp is turned off, and the outer ice-water mixture is cleaned to obtain an oily solution.

[0153] Then, the oily liquid after the reaction is filled with an inert gas such as argon (Ar) and then sealed and left to stand until the temperature returns to about 25°C at room temperature. The obtained substance is then heated in a rare gas environment (the heating temperature is 120°C to 130°C, and the rare gas is continuously ventilated during this period) for 1.5h to 2h to remove excess solvents, newly generated volatile impurities, and other gas impurities. Thus, a silicon precursor is obtained, with the chemical formula S(SiHROH)2.

[0154] The reaction equation involved in preparing the silicon precursor in step S100 is as follows:

[0155]

[0156] In the above reaction equation, HCOOH represents formic acid, and UV represents ultraviolet light.

[0157] The silicon precursor is mainly composed of Si-O and Si-R combinations; under this structure, the spatial structure of the ion channel can be stretched very wide, and metal ions of all sizes, such as Pd cations, can pass through.

[0158] S200, preparing an organosiloxane polymer from a silicon precursor, specifically comprising:

[0159] The silicon precursor, the organic solvent and the catalyst are uniformly mixed, and the temperature and pressure are increased to the second temperature and the first pressure in an inert gas atmosphere to react. After the reaction is completed, the temperature and pressure are decreased to the third temperature and the second pressure in an inert gas atmosphere, and separated to obtain an organosiloxane polymer.

[0160] Optionally, the molar ratio of the silicon precursor, the organic solvent and the catalyst is 1: (12-20): (0.4-0.85). Further, the molar ratio of the silicon precursor, the organic solvent and the catalyst is 1: (14-18): (0.5-0.7). For example, the molar ratio of the silicon precursor, the organic solvent and the catalyst can be 1: 12: 0.4, 1: 14: 0.5, 1: 15: 0.5, 1: 16: 16, 1: 18: 0.7, 1: 20: 0.85, etc. The silicon precursor is the silicon precursor prepared by step S100.

[0161] The above-mentioned ratio, that is, the amount of silicon precursor, organic solvent and catalyst added can be adjusted according to the specific usage and the specific progress of the reaction to optimize the amount of addition, reduce side reactions, increase yield and reduce costs.

[0162] Optionally, the temperature increase rate is 1-5°C / h, and the pressure increase rate is 0.04-0.08atm / h; further, the temperature increase rate is 2-4°C / h, and the pressure increase rate is 0.05-0.06atm / h. For example, the temperature increase rate may be 1°C / h, 2°C / h, 3°C / h, 4°C / h, 5°C / h, etc.; the pressure increase rate may be 0.04atm / h, 0.05atm / h, 0.06atm / h, 0.07atm / h, 0.08atm / h, etc.

[0163] Optionally, the temperature reduction rate is 0.5-5°C / h, and the pressure reduction rate is 0.02-0.08atm / h; the temperature reduction rate is 1-4°C / h, and the pressure reduction rate is 0.03-0.06atm / h. For example, the temperature reduction rate may be 0.5°C / h, 1°C / h, 2°C / h, 3°C / h, 4°C / h, 5°C / h, etc.; the pressure reduction rate may be 0.02atm / h, 0.04atm / h, 0.05atm / h, 0.06atm / h, 0.07atm / h, 0.08atm / h, etc.

[0164] It is worth noting that in the above step S200, during the preparation of the organosiloxane polymer, the reaction environment needs to be strictly controlled, and the rate of temperature increase and pressure increase and the rate of temperature reduction and pressure reduction should not be too fast, otherwise it will be easy to cause side reactions, affecting the formation of the product. This embodiment can reduce the occurrence of side reactions as much as possible and improve the product yield by controlling the temperature increase and pressure increase rate and the temperature reduction and pressure reduction rate within the above range. In addition, during the reaction process, it is necessary to pass a rare gas such as argon to avoid the introduction of impurities.

[0165] In addition, the gases generated during the reaction, such as a small amount of water vapor, organic solvents, and volatile products such as H2S, need to be washed out by continuous flow of rare gas before and after the reaction to avoid affecting the reaction.

[0166] Optionally, the second temperature is 120°C to 180°C, and the first pressure is 1.0atm to 3.0atm; further, the second temperature is 130°C to 160°C, and the first pressure is 1.0atm to 2.0atm. For example, the second temperature may be 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, etc., and the first pressure may be 1.0atm, 1.5atm, 2atm, 2.5atm, 3.0atm, etc. The second temperature and the first pressure are the reaction temperature and pressure. By controlling the reaction temperature and pressure within the above range, the condensation reaction is carried out under high temperature and pressure conditions, so that the reaction can proceed more smoothly and the reaction rate is faster.

[0167] Optionally, the third temperature may be normal temperature, and the second pressure may be normal pressure, such as the third temperature is 22°C to 28°C, and the second pressure is 0.9atm to 1.1atm; further, the third temperature may be 22°C, 24°C, 25°C, 26°C, or 28°C; and the second pressure is 1atm.

[0168] Optionally, the reaction time at the second temperature and the first pressure is 70 hours to 100 hours, that is, the reaction time is at least 70 hours, such as 70 hours to 100 hours; further, the reaction time is 75 hours to 90 hours. For example, the reaction time can be 70 hours, 75 hours, 80 hours, 85 hours, 90 hours, 100 hours, etc.

[0169] In step S200, the silicon precursor prepared and purified in step S100 is subjected to a condensation reaction to remove H2S and H2O in a rare gas atmosphere and a second temperature (high temperature) environment. The S-Si bond and Si-H bond of the silicon precursor are broken, and the aforementioned generated substance is heated and pressurized in a rare gas environment (e.g., the temperature is within the range of 120 to 180°C and the pressure is within the range of 1 to 3 atm), and then, under the catalysis of a catalyst, the silicon precursor undergoes the aforementioned self-polymerization reaction to generate a high polymer silane, that is, an organic siloxane polymer.

[0170] Exemplarily, the step of preparing an organosiloxane polymer from a silicon precursor in S200 specifically includes:

[0171] According to the order and ratio, the silicon precursor, organic solvent and catalyst obtained in step S100 are added to the container in sequence, and argon is introduced into the device for 1 to 5 minutes (the pressure is controlled within the range of 1.0 atm to 3.0 atm), and then the temperature is slowly raised to 120°C to 180°C, and then the temperature is stopped for reaction; after the temperature is stopped, the temperature is maintained for at least 70 hours for reaction. After the heating reaction is completed, the temperature and pressure are slowly lowered while the argon is kept introduced (for removing volatile impurities) until the third temperature and the second pressure are restored, that is, the room temperature and normal pressure (1 atm, about 25°C). The obtained substance is then allowed to stand and filtered (to remove solid impurities) to obtain an organosiloxane polymer.

[0172] The equation involved in preparing the organosiloxane polymer from the silicon precursor in step S200 is as follows:

[0173]

[0174] In this reaction equation, Ar represents argon gas.

[0175] Reference Figure 1 It can be seen that the prepared organosiloxane polymer connects multiple levels through the Si-O skeleton and the series-parallel connection between the R groups to form a spatial network three-dimensional structure. As an example, the organosiloxane includes a multi-layer planar tetragonal grid layer, and these multi-layer planar tetragonal grid layers can be connected in series and parallel through the R group to form an organosiloxane with a spatial network three-dimensional structure. The interlayer spacing of the three-dimensional multilayer structure is longer than the CC bond in the graphite structure due to the Si-O and / or Si-R combination, and the interlayer spacing is larger than that of the ordinary graphite layer structure. At the same time, the intralayer holes of the Si-O and / or Si-R layers will also widen the gaps between the layers. These two parts constitute the pathways of / electrons / side reaction products in the organosilicon material-ion and electron conduction, and the side reaction products are separated to prevent accumulation and expansion.

[0176] also, Figure 3 , Figure 4 The NMR spectrum (ChemNMR) of the reactants (raw materials) used in the preparation of the above-mentioned organosiloxane polymer is shown. 1 H Estimation), such as Figure 3 The NMR spectrum of one of the reactants (SiH2ROH) is shown (frequency 400 Hz, deuterated reagents include dimethyl sulfoxide DMSO, deuterated chloroform CDCl3), Figure 4The NMR diagram of another reactant (SiH2RSH) is shown - hydrogen spectrum (frequency 400Hz, deuterated reagents include dimethyl sulfoxide DMSO, deuterated chloroform CDCl3). Figure 3 , Figure 4 As can be seen, the molecular structures of the above two reactants were confirmed using hydrogen spectrum, showing the molecular structures of the two reactants SiH2ROH and SiH2RSH provided.

[0177] The synthesis and preparation method of the organosiloxane polymer provided in this embodiment is simple, the environment is easy to be artificially controlled, and it is less toxic and has a low risk factor, which can provide convenience for mass production.

[0178] In some other embodiments, the preparation of an organosiloxane polymer having a cage structure specifically includes:

[0179] Two different organosilicon precursors RSi(OH)3 and [RSi(OH)2]2O were synthesized respectively;

[0180] The two synthesized organosilicon precursors RSi(OH)3 and [RSi(OH)2]2O are then mixed to synthesize an organosiloxane polymer with a cage-type structure.

[0181] As an example, the chemical equation involved in the preparation of an organosiloxane polymer having a cage structure is shown below:

[0182]

[0183] Among them, R is preferably at least one of tert-butyl or tert-hexyldimethylsilyl chloride.

[0184] In this chemical equation, aniline represents aniline, H2O represents water, ether represents ethyl ether, KOH represents potassium hydroxide, SiO2 represents silicon dioxide, ethanol represents ethanol, DCC represents N,N'-dicyclohexylcarbodiimide, DMSO represents dimethyl sulfoxide, and DMF represents dimethylformamide.

[0185] Optionally, the preparation of the silicon precursor RSi(OH)3 includes: uniformly mixing reactants, an organic solvent and a catalyst, reacting at a temperature ≤30°C, filtering and distilling after the reaction to obtain the silicon precursor RSi(OH)3. The reactants include RSiCl3.

[0186] As an example, the preparation of the silicon precursor RSi(OH)3 specifically includes: injecting the reactants and organic solvents such as ethanol into a flask according to the prescribed ratio and stirring for 15 to 25 minutes (controlling the temperature below 25°C to reduce the volatilization of the raw materials) until they are evenly mixed; after stirring evenly, adding a catalyst such as aniline according to the prescribed ratio (controlling the temperature below 25°C); then adding an excess of deionized water, the reaction begins (minimizing the side reaction of reverse hydrolysis); after a period of time, the reaction ends. Then, the liquid after the reaction is filtered (to remove solid impurities), allowed to stand, and separated (the lower layer of oily liquid is taken) for preliminary purification; then the obtained substance is subjected to low-temperature and low-pressure distillation (controlling the gas pressure below 1Atm and the temperature below 80°C) to achieve the purpose of removing organic solvents, newly generated volatile substances, excess water vapor and other gas impurities. In this way, a silicon precursor crystal can be obtained.

[0187] Optionally, the preparation of the silicon precursor [RSi(OH)2]2O includes: uniformly mixing reactants, an organic solvent, a catalyst and Si2O, reacting at a temperature ≤30°C, filtering and distilling after the reaction to obtain the silicon precursor [RSi(OH)2]2O. The reactants include RSiCl3.

[0188] A small amount of SiO2 is added during the preparation of the silicon precursor to supplement Si. The reason for supplementing Si is that side reactions may occur, resulting in silicon loss. A small amount of SiO2 (such as not more than 1.5%) is added until it no longer decreases, indicating that Si supplementation is completed and the addition can be stopped.

[0189] As an example, the specific preparation of the silicon precursor [RSi(OH)2]2O includes: first, the raw materials and organic solvents such as ether are injected into a flask according to the prescribed ratio and stirred for 15 to 25 minutes (control the temperature below 25°C) until they are evenly mixed; after stirring evenly, a catalyst such as KOH is added according to the prescribed ratio (control the temperature below 30°C), and a small amount of SiO2 (for Si supplementation) is added at the same time, and then an excess of deionized water is added, and the reaction begins; after a period of time, the reaction ends. Then, the liquid after the reaction is filtered (to remove solid impurities), allowed to stand, and separated (the lower layer of oily liquid is taken) for preliminary purification; then the obtained substance is subjected to low-temperature and low-pressure distillation (control the gas pressure below 1Atm and the temperature below 80°C) to achieve the purpose of removing organic solvents, newly generated volatile substances, excess water vapor and other gas impurities. In this way, a silicon precursor crystal can be obtained.

[0190] In the embodiments of the present application, during the preparation of silicon precursor RSi(OH)3 and silicon precursor [RSi(OH)2]2O, the molar ratio of reactant, organic solvent and catalyst is (4-8): (15-30): (0.5-2). Further, the molar ratio of reactant, solvent and catalyst is (1.5-8): (16-27): (0.8-1.6).

[0191] It should be noted that the organic solvent and catalyst used in the preparation of the organosiloxane polymer having a cage structure and the preparation of the organosiloxane polymer having a planar tetragonal lattice structure may be the same or similar. As an example, in the preparation of the organosiloxane polymer having a cage structure, the organic solvent includes but is not limited to at least one of dimethyl sulfoxide, N,N-dimethylformamide, a thiol-containing compound, an alcohol solvent or an ether solvent. The catalyst includes but is not limited to at least one of propylene glycol methyl ether acetate, N,N'-dicyclohexylcarbodiimide, aniline or potassium hydroxide.

[0192] Furthermore, the operation method or precautions for preparing organosiloxane using silicon precursor RSi(OH)3 and silicon precursor [RSi(OH)2]2O can also be the same or similar to the above-mentioned preparation of organosiloxane polymers with a planar tetragonal lattice structure, and will not be described in detail here. As an example, the preparation of an organosiloxane polymer with a cage structure includes: adding the material crystals of the two precursors synthesized above, an organic solvent such as DMF, and a catalyst such as DCC in a container in order and material proportion; slowly heating after passing 1 to 5 minutes of Ar gas in the device, and stopping the heating at 110 to 150°C. After stopping the heating, keep this temperature and continue heating for at least 90 hours. After the heating is completed, keep passing Ar gas (argon gas) (remove volatile impurities) while slowly cooling until it returns to room temperature (about 25°C); let the obtained material stand and filter (remove solid impurities) to obtain an organosiloxane polymer. It should be noted that this reaction environment requires relatively strict control, and the speed of heating and cooling should not be too fast to reduce the occurrence of side reactions. During the reaction, a rare gas (such as Ar) needs to be introduced to prevent the introduction of impurities. The gases produced by the reaction (a small amount of water vapor, organic solvents, volatile products) need to be washed out by continuous flow of rare gas (Ar) before and after the reaction.

[0193] Depend on Figure 2 It can be seen that the organosiloxane polymer with a cage structure connects the cage cubes one by one through the series and parallel connection between the R groups to form a three-dimensional structure. The gaps between the cage cubes constitute the path of ions / electrons / side reaction products - ions and electrons conduct electricity, and the side reaction products are separated to prevent accumulation and expansion.

[0194] also, Figure 5 , Figure 6The NMR diagram of the reactants (raw materials) used in the preparation of the above-mentioned organosiloxane polymer is shown, such as, Figure 5 The NMR graph of the reactant (RSiCl3) -C spectrum (frequency 400Hz, deuterated reagents include deuterated chloroform CDCl3), Figure 6 The NMR diagram of the reactant (RSiCl3) -H spectrum (frequency 400 Hz, deuterated reagents include deuterated chloroform CDCl3). Figure 5 and Figure 6 In the formula, C4H9Cl3Si represents isobutyltrichlorosilane. Figure 5 , Figure 6 As can be seen, the molecular structures of the above reactants were confirmed by carbon spectrum and hydrogen spectrum respectively.

[0195] Furthermore, the prepared organosiloxane polymer, that is, the above-mentioned organosiloxane polymer with a planar tetragonal lattice structure or a cage-type structure, is applied to the negative electrode active material of a lithium-ion battery, and a step of forming a carbon coating layer on the surface of the organosiloxane polymer comprises: using the prepared organosiloxane polymer as a matrix material, and adopting an atomic layer deposition (ALD) process to form a carbon coating layer on the surface of the organosiloxane polymer.

[0196] Atomic layer deposition (ALD) is a technique that deposits materials on the surface of a material layer by layer in the form of a single atomic film based on chemical vapor. Two or more precursor chemicals containing different elements of the deposited material are introduced to the surface of the material one at a time. Each precursor can saturate the surface of the material to form a single layer of material.

[0197] In this embodiment, a carbon coating layer is formed on the surface of the organosiloxane polymer by atomic layer deposition technology, which has the advantages of high precision, excellent three-dimensional conformality, high flatness, excellent adhesion, low thermal budget (low deposition temperature), etc. For example, it can simply and accurately control the thickness of the substrate film by controlling the reaction cycle, and the thickness accuracy of the film can reach the thickness of one atom, with high precision. A film with the same shape as the original substrate can be generated, that is, the film can be uniformly deposited on a surface similar to a concave surface; therefore, it can be applied to substrates of different shapes; uniform three-dimensional film, shape consistent with the original, conformality, is the unique advantage of ALD technology. There are no pinholes on its surface, and the bottom-up growth mechanism determines the pinhole-free nature of the film, which is valuable for blocking and passivation applications, and has high flatness. The chemical adsorption of its precursor to the substrate surface ensures excellent adhesion. This process technology can grow thin films at low temperatures (room temperature to 400°C), which is very attractive for polymer devices and biomaterial coatings with temperature restrictions.

[0198] Specifically, the step of forming a carbon coating layer on the surface of the organosiloxane polymer comprises the following steps:

[0199] A carrier gas is introduced into the atomic layer deposition device, the organosiloxane polymer is placed in the atomic layer deposition device, the first gas phase carbon source is introduced, and the first gas phase deposition is performed after heating to perform the first stage of carbon coating on the surface of the organosiloxane polymer. The carrier gas can be an inert gas such as argon; the heating temperature is 20°C to 40°C, and the heating time is 2h to 5h; further, the heating temperature is 25°C to 35°C, and the heating time is 3h to 4h. For example, the heating temperature can be 25°C, 30°C, 35°C, 40°C, etc.; the heating time can be 2h, 3h, 4h, 5h, etc.

[0200] Then, an inert gas such as argon is introduced to wash out the remaining waste gas, and then the temperature is lowered, such as slowly lowering the temperature to the temperature before heating, and then a second gas phase carbon source is introduced, and a second gas phase deposition is performed after heating to perform a second stage of carbon coating on the surface of the organosiloxane polymer, and a carbon coating layer is formed on the surface of the organosiloxane polymer to obtain a lithium ion battery negative electrode active material including an organosiloxane polymer and a carbon coating layer. Among them, the cooling temperature is ≤20°C, and the cooling time is 3h to 6h. For example, the cooling temperature can be 20°C, 18°C, etc.; the cooling time can be 3h, 4h, 5h, 6h, etc.

[0201] Optionally, the first gas-phase carbon source is recorded as C1, the second gas-phase carbon source is recorded as C2, and C1 and C2 satisfy the following relationship:

[0202] (1) Unsaturation: 2≤C1≤C2≤6;

[0203] (2) Gas flow rate (based on the amount of the organosiloxane polymer (base material) as 1 eq): 1 eq ≤ C1 ≤ C2 ≤ 4 eq.

[0204] Therefore, by setting the first gas-phase carbon source and the second gas-phase carbon source, the coated material layer can be made smoother and more precise.

[0205] Exemplarily, the step of forming a carbon coating layer on the surface of the organosiloxane polymer specifically includes:

[0206] (1) An atomic layer deposition (ALD) device is filled with a carrier gas such as argon, and a coated substrate is provided, such as a substrate subjected to ozone treatment for about 15 minutes, and then coated with an organic siloxane polymer to serve as a substrate.

[0207] (2) Filling the first gas-phase carbon source C1 into the ALD device.

[0208] (3) Slowly increase the temperature by 20°C to 40°C (for 2h to 5h) to activate the coating carbon source. The first stage of coating begins, and the first vapor deposition is performed to form the first layer of high-quality thin film coating.

[0209] (4) After step (3) is completed, an inert gas such as argon is introduced to wash out the remaining waste gas, and then the temperature is lowered, such as slowly lowering the temperature to the temperature before the heating.

[0210] (5) charging the second gas-phase carbon source C2 into the ALD device;

[0211] (6) As in step (3), the coating carbon source is activated and the second stage of coating begins to form a high-shape-retaining coating film.

[0212] (7) Repeat step (4) to wash out the remaining waste gas.

[0213] (8) After ALD carbon coating is completed, an organic-inorganic composite silicon-carbon material is obtained, that is, a lithium-ion battery negative electrode active material including an organic siloxane polymer and a carbon coating layer is obtained.

[0214] It should be noted that in the embodiment of the present application, the ALD deposition technology is preferably used for coating the carbon coating layer, but it is not limited to this. For example, when the material of the carbon coating layer adopts traditional graphite, soft carbon, hard carbon and other materials, other methods can also be used to coat the traditional carbon material on the surface of the organic silicone polymer to form a carbon coating layer, which will not be described in detail here.

[0215] 2. Negative electrode

[0216] In some embodiments, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode active material layer includes the aforementioned negative electrode active material for lithium-ion batteries.

[0217] As an example, the negative electrode current collector has two surfaces facing each other in its thickness direction, and the negative electrode active material layer is disposed on either or both of the two facing surfaces of the negative electrode current collector.

[0218] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, the composite current collector includes, but is not limited to, copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, etc. Alternatively, the negative electrode current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.). In some embodiments, the negative electrode current collector is a copper foil.

[0219] In some embodiments, the negative electrode active material layer may further include a binder. The binder may include various binder polymers, for example, at least one selected from styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).

[0220] In some embodiments, the negative electrode active material layer may further include a conductive agent. The conductive agent may use any conductive material as the conductive material as long as it does not cause chemical changes. For example, the conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0221] In some embodiments, the negative electrode active material layer may further include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0222] The method for preparing the negative electrode sheet is a method for preparing the negative electrode sheet that can be used for an electrochemical device and is well known in the art. Exemplarily, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material of a lithium-ion battery, a conductive agent, a binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0223] In some embodiments, the structure of the negative electrode sheet is a negative electrode sheet structure known in the art and can be used in electrochemical devices.

[0224] 3. Battery

[0225] In some embodiments, a battery is provided, the battery comprising a positive electrode plate, a negative electrode plate, an electrolyte and a separator. Optionally, the battery may be a secondary battery, and the secondary battery may be a lithium ion battery or a sodium ion battery.

[0226] The main feature of the battery is that it includes any of the above-mentioned lithium-ion battery negative electrode active materials of the present application. Due to the use of the lithium-ion battery negative electrode active material of the present embodiment, the probability of secondary battery side reactions can be reduced, the expansion rate of the negative electrode plate of the battery can be reduced, or the deterioration of the negative electrode of the battery can be reduced, thereby improving the cycle life of the battery.

[0227] In this embodiment, the structure of the positive electrode plate and the structure of the isolation membrane may be the positive electrode plate structure and the isolation membrane structure known in the art and can be used for secondary batteries, and are not limited to this and will not be described in detail here.

[0228] The specific type and structure of the electrolyte may be any electrolyte type known in the art that can be used in secondary batteries, and is not limited thereto and will not be described in detail herein.

[0229] IV. Application

[0230] The use of the secondary battery of the present application is not particularly limited, and the secondary battery can be applied to any electrical device known in the prior art.

[0231] Exemplarily, an embodiment of the present application further provides an electrical device, which includes at least one of the secondary battery, battery module and battery pack of the present application. The secondary battery, battery module and battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device can be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.

[0232] The electric device can select a secondary battery, a battery module or a battery pack according to its usage requirements.

[0233] Example

[0234] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific technology or conditions are specified in the embodiments, the technology or conditions described in the literature in this area or the product instructions are used. If the manufacturer of the reagents, materials or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0235] Example 1

[0236] The preparation of the negative electrode active material of the lithium ion battery comprises the following steps:

[0237] S100, preparation of silicon precursor:

[0238] According to the ratio, SiH2ROH, SiH2RSH and organic solvent DMSO are added to the flask and mixed, and stirred for 2 minutes until the mixture is uniform; after stirring and mixing uniformly, the catalyst PGMEA and the auxiliary agent HCOOH are added according to the ratio at room temperature, and then a large container is placed outside the flask, and a large amount of crushed ice and water mixture is added to the large container to maintain the ambient temperature at about 0°C; then, the mixture in the flask is irradiated with ultraviolet light through the reserved UV irradiation hole / surface, and the reaction begins. After a period of reaction, such as 40 minutes, the reaction ends, the ultraviolet lamp is turned off and the outer ice-water mixture is cleaned to obtain an oily solution. Then, the reacted oily liquid is filled with argon and sealed and left to stand until it returns to room temperature of about 25°C, and then the obtained substance is heated in a rare gas environment (the heating temperature is 125°C, and the rare gas is ventilated during the period) for 1.5 hours. Thus, a silicon precursor with the chemical formula S(SiHROH)2 is obtained.

[0239] Among them, the R group is ethyl; the molar ratio of the sum of the amounts of the first reactant and the second reactant to the auxiliary agent, the organic solvent and the catalyst is 7.2:3.9:24:0.42, and the molar ratio of the first reactant to the second reactant is 3.5:3.7.

[0240] S200, Preparation of organosiloxane polymer from silicon precursor:

[0241] Connect a reaction device with a rare gas environment such as argon that can be heated, and add the silicon precursor, organic solvent DMSO and catalyst DCC obtained in step S100 to the container in order and proportion. After passing argon for 2 minutes in the device, slowly heat it to 140°C and increase the pressure to 2.8atm. The heating rate is 4°C / h and the pressure increase rate is 0.06atm / h. After stopping the temperature and pressure increase, keep the temperature and pressure for 78 hours. After the heating reaction is completed, keep passing argon while slowly cooling and reducing the pressure. After about 50 hours, return to 25°C and 1atm. Then seal the obtained substance and let it stand for 2 hours before filtering, and then seal it with rare gas to obtain an organosiloxane polymer.

[0242] Among them, the molar ratio of silicon precursor, organic solvent and catalyst is 1:14:0.8.

[0243] S300, Atomic layer deposition to prepare carbon coating:

[0244] (1) Fill the atomic layer deposition (ALD) device with argon gas, set up the coated substrate, such as treating the substrate with ozone for about 15 minutes, and then coating the organic siloxane polymer to serve as the substrate. (2) Fill the ALD device with a first gas phase carbon source C1 with a flow rate of 1.2eq. (3) Slowly increase the temperature by 20°C (time is 2h) to activate the coated carbon source, start the first stage of coating, and perform the first gas phase deposition to form the first layer of high-quality thin film coating. (4) After step (3) is completed, introduce argon gas again to wash out the remaining waste gas, and then cool down, such as slowly cooling to the temperature before heating. (5) Fill the ALD device with a second gas phase carbon source C2 with a flow rate of 3.0eq. (6) As in step (3), activate the coated carbon source, start the second stage of coating, and form a high-conformity coating film. (7) Repeat step (4) to wash out the remaining waste gas. (8) After ALD carbon coating is completed, an organic-inorganic composite silicon-carbon material is obtained, that is, a lithium-ion battery negative electrode active material including an organic siloxane polymer and a carbon coating layer is obtained.

[0245] The first gas-phase carbon source C1 is a mixed gas composed of CO+C2H2 in a volume ratio of 1:2; the second gas-phase carbon source C2 is C4H4O.

[0246] Example 2

[0247] The preparation of the negative electrode active material for the lithium ion battery is the same as that in Example 1, except that the R group is tert-butyl.

[0248] Example 3

[0249] The preparation of the negative electrode active material for the lithium ion battery is the same as that in Example 1, except that the R group is a phenyl group.

[0250] Example 4

[0251] The preparation of the negative electrode active material for a lithium ion battery is the same as that in Example 1, except that the molar ratio of the sum of the amounts of the first reactant and the second reactant to the auxiliary agent, the organic solvent and the catalyst is 6:3:25:0.35.

[0252] Example 5

[0253] The preparation of the negative electrode active material for a lithium ion battery is the same as that in Example 1, except that the molar ratio of the sum of the amounts of the first reactant and the second reactant to the auxiliary agent, the organic solvent and the catalyst is 2.5:1.5:22:0.05.

[0254] Example 6

[0255] The preparation of the negative electrode active material of the lithium ion battery is the same as that of Example 1, except that: the carbon coating layer is prepared by coating method. The carbon coating layer of this embodiment adopts the coating form of secondary particles.

[0256] Example 7

[0257] The preparation of the negative electrode active material of the lithium ion battery is the same as that in Example 1, except that when preparing the organosiloxane polymer, argon gas is introduced into the device for 2 minutes and then the temperature is slowly raised to 160°C.

[0258] Example 8

[0259] The preparation of the negative electrode active material of the lithium ion battery is the same as that in Example 1, except that when preparing the organosiloxane polymer, the heating rate is 5° C. / h and the pressure increase rate is 1.0 atm / h.

[0260] Example 9

[0261] The preparation of the negative electrode active material of the lithium ion battery comprises the following steps:

[0262] S110, preparation of silicon precursor RSi(OH)3:

[0263] According to the ratio, inject 5 mol RSiCl3 and 16 mol ethanol into the flask and stir for 25 minutes (control the temperature at 20°C) until it is evenly mixed. After stirring evenly, add 1.3 mol of aniline (control the temperature at 20°C), and then add 10 mol of deionized water. After the temperature in the container no longer changes, the reaction is over. Then, filter the liquid obtained after the reaction (to remove solid impurities), let it stand for 10 minutes, and separate the liquid (take the lower layer of oily liquid). Then, distill the obtained substance at low temperature and low pressure (0.8→0.2Atm, 65→25°C) to remove impurities from the product. Thus, the silicon precursor RSi(OH)3 is obtained.

[0264] Among them, the R group is tert-butyl (t-Bu).

[0265] S120, preparation of silicon precursor [RSi(OH)2]2O:

[0266] According to the ratio, 5 mol RSiCl3 and 16 mol ether are injected into the flask and stirred for 25 minutes (control the temperature at 20°C) until the mixture is evenly mixed. After stirring evenly, 1.3 mol KOH is added (control the temperature below 30°C). Then, 10 mol deionized water and 0.05 mol SiO2 are added until the temperature in the container no longer changes, and the reaction is completed. Then, the liquid obtained after the reaction is filtered (to remove solid impurities), allowed to stand for 10 minutes, and separated (the lower layer of oily liquid is taken); then, the obtained substance is subjected to low-temperature and low-pressure distillation (0.8→0.2Atm, 65→25°C) to remove impurities from the product. Thus, the silicon precursor [RSi(OH)2]2O is obtained.

[0267] Among them, the R group is tert-butyl (t-Bu).

[0268] S200, Preparation of organosiloxane polymer from silicon precursor:

[0269] Connect a reaction device with a rare gas environment that can be heated, such as argon, and add the silicon precursors RSi(OH)3 and [RSi(OH)2]2O, organic solvent DMF and catalyst DCC obtained above to the container in order and proportion. After passing argon gas for 2 minutes, slowly heat it to 120°C and then stop heating. The heating rate is 5°C / h. After stopping heating, keep the temperature and continue heating for 96 hours. After the heating reaction is completed, keep passing argon gas (to remove volatile impurities) while slowly cooling down, and return to about 25°C after about 72 hours. Then seal the obtained substance and let it stand for 12 hours before filtering to obtain an organosiloxane polymer.

[0270] S300, Atomic layer deposition to prepare carbon coating:

[0271] (1) Fill the atomic layer deposition (ALD) device with argon gas and set up a coated substrate, such as coating an organic siloxane polymer as a substrate. (2) Fill the ALD device with a first gas phase carbon source C1 with a flow rate of 1.2eq. (3) Slowly increase the temperature by 20°C (time is 2.5h) to activate the coated carbon source, and the first stage of coating begins. The first gas phase deposition is performed to form the first layer of high-quality thin film coating. (4) After step (3) is completed, argon gas is introduced again to wash out the remaining waste gas, and then the temperature is lowered, such as slowly cooling (3h) to the temperature before heating. (5) Fill the ALD device with a second gas phase carbon source C2 with a flow rate of 3.0eq. (6) As in step (3), activate the coated carbon source, and the second stage of coating begins to form a high-conformity coating film. (7) Repeat step (4) to wash out the remaining waste gas. (8) After ALD carbon coating is completed, an organic-inorganic composite silicon-carbon material is obtained, that is, a lithium-ion battery negative electrode active material including an organic siloxane polymer and a carbon coating layer is obtained.

[0272] The first gas-phase carbon source C1 is a mixed gas composed of CO+C2H2 in a volume ratio of 1:1; the second gas-phase carbon source C2 is C4H4O.

[0273] Example 10

[0274] The preparation of the negative electrode active material of the lithium ion battery is the same as that in Example 9, the difference is that in the process of preparing the silicon precursor RSi(OH)3 and the process of preparing the silicon precursor [RSi(OH)2]2O, the molar ratio of the reactant, the organic solvent and the catalyst is 8:27:1.6.

[0275] Embodiment 11

[0276] The preparation of the negative electrode active material of the lithium ion battery is the same as that in Example 9, the difference is that in the process of preparing the silicon precursor RSi(OH)3 and the silicon precursor [RSi(OH)2]2O, the molar ratio of the reactant, the organic solvent and the catalyst is 4.5:16:0.8.

[0277] Comparative Example 1

[0278] The negative electrode active material of lithium-ion batteries uses existing inorganic silicon materials (SiOx).

[0279] Comparative Example 2

[0280] The negative electrode active material of lithium-ion batteries adopts existing graphite materials.

[0281] The negative electrode sheets were made of the negative electrode active materials of lithium ion batteries prepared in the above embodiments and comparative examples, and button batteries were assembled to test and analyze their electrochemical performance, as follows:

[0282] (1) Preparation of negative electrode sheet: The negative electrode active materials of the lithium ion battery of the above-mentioned embodiments and comparative examples, the conductive agent conductive carbon black, the binder polyvinylidene fluoride and the solvent are uniformly mixed in a mass ratio of 6:2:1:1 to form a negative electrode slurry, and the negative electrode slurry is coated on the negative electrode current collector aluminum foil. After drying, cold pressing and other processes, a negative electrode sheet is obtained.

[0283] (2) Preparation of batteries:

[0284] A pole piece containing lithium nickel cobalt manganese oxide as an active material is used as a positive pole piece, LiPF6 / EC+DEC (volume ratio 1:1) is used as an electrolyte, an ordinary commercial diaphragm PP / PE is used as an isolation membrane, and the aforementioned negative pole piece is used as a negative pole piece, and a CR2032 button battery is assembled in a glove box.

[0285] Performance Testing

[0286] Battery cycle life performance test, test methods include:

[0287] The batteries prepared in the above embodiments and comparative examples were charged to 4.4V at 0.2C constant current and constant voltage at a constant temperature of 25°C, with a cut-off current of 0.05C; and then discharged to 2.8V at 0.2C. The charge and discharge cycles were continued according to the above steps until the capacity retention rate of the battery reached 80%, and the cycle number of the battery was recorded (when the cycle number was less than this number, the capacity retention rate was not less than 80%), and the capacity retention rate = discharge capacity of the Nth cycle / discharge capacity of the first cycle.

[0288] The test results are shown in Table 1 below.

[0289] Table 1

[0290] Group Capacity retention rate (500 cycles comparison) Example 1 92.3% Example 2 91.2% Example 3 91.1% Example 4 91.0% Example 5 90.6% Example 6 90.5% Example 7 90.3% Example 8 90.1% Example 9 90.4% Example 10 90.3% Embodiment 11 90.2% Comparative Example 1 90.0% Comparative Example 2 89.9%

[0291] It can be seen from the data in Table 1 that, compared with the existing lithium ion battery negative electrode active materials of Comparative Examples 1 and 2, the lithium ion battery negative electrode active materials prepared in Examples 1-11 of the present invention have better capacity retention during the charge and discharge process, thereby improving the cycle performance of the battery.

[0292] Parts of the present invention that are not described in detail are well known to those skilled in the art.

[0293] The basic principle of the present invention is described above in conjunction with specific embodiments. However, it should be pointed out that the advantages, strengths, effects, etc. mentioned in the present invention are only examples and not limitations, and it cannot be considered that these advantages, strengths, effects, etc. must be possessed by each embodiment of the present invention. In addition, the specific details disclosed above are only for the purpose of illustration and facilitation of understanding, rather than limitation, and the above details do not limit the present invention to being implemented by adopting the above specific details.

[0294] It should be noted that the term "and / or" or " / " used in this document is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. The singular forms of "a", "the" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0295] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0296] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A lithium ion battery negative electrode active material, characterized in that: include: A silicon-based material, and a carbon coating layer coated on the surface of the silicon-based material; The silicon-based material is an organosiloxane polymer, and the organosiloxane polymer includes a Si-O group and a Si-R group; Among them, R is selected from at least one of ethyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, decyl, tert-hexyldimethylchlorosilane, substituted or unsubstituted C6-16 cycloalkyl, substituted or unsubstituted C6-16 aryl, and substituted or unsubstituted C8-16 aralkyl.

2. The negative electrode active material for lithium-ion batteries according to claim 1, characterized in that: The organosiloxane polymer comprises a group represented by the following formula (I): Formula I; Among them, the value of n is 2 to 10000.

3. The negative electrode active material for lithium-ion batteries according to claim 1, characterized in that: The organosiloxane polymer has a planar polygonal network structure, or the organosiloxane polymer has a cage structure.

4. The negative electrode active material for lithium-ion batteries according to claim 3, characterized in that: The number average molecular weight of the organosiloxane polymer is ≤100,000.

5. The negative electrode active material for lithium ion batteries according to any one of claims 1 to 4, characterized in that: The material of the carbon coating layer includes at least one of natural graphite, artificial graphite, soft carbon, hard carbon, graphene, carbon nanotubes, mesophase carbon microspheres or carbon fibers.

6. The negative electrode active material for lithium ion batteries according to any one of claims 1 to 4, characterized in that: The carbon coating layer is formed by gas-phase coating of at least two gas-phase carbon sources; Wherein, the gas-phase carbon source includes a first gas-phase carbon source and a second gas-phase carbon source, the first gas-phase carbon source and the second gas-phase carbon source include unsaturated compounds containing alkenyl or alkynyl groups and having no more than 6 carbon atoms, and the first gas-phase carbon source and the second gas-phase carbon source satisfy the following relationship: 2≤the unsaturation degree of the first gas-phase carbon source≤the unsaturation degree of the second gas-phase carbon source≤6.

7. A method for preparing a negative electrode active material for a lithium ion battery, characterized in that: include: preparing a silicon precursor; The silicon precursor is used to prepare an organosiloxane polymer, wherein the prepared organosiloxane polymer includes a Si-O group and a Si-R group; wherein R is selected from at least one of ethyl, n-butyl, isobutyl, sec-butyl, tert-butyl, hexyl, octyl, decyl, tert-hexyldimethylchlorosilane, substituted or unsubstituted C6-16 cycloalkyl, substituted or unsubstituted C6-16 aryl, and substituted or unsubstituted C8-16 aralkyl; A carbon coating layer is formed on the surface of the organosiloxane polymer to prepare a lithium ion battery negative electrode active material comprising a core of the organosiloxane polymer and a carbon coating layer formed on the outer surface of the organosiloxane polymer.

8. The method for preparing the negative electrode active material for lithium ion batteries according to claim 7, characterized in that: The preparation of the silicon precursor specifically comprises: The reactants, organic solvent and catalyst are mixed uniformly and reacted, and impurities are removed after the reaction is completed to obtain the silicon precursor; The silicon precursor is S(SiHROH)2; Alternatively, the silicon precursor is RSi(OH)3 and [RSi(OH)2]2O.

9. The method for preparing the negative electrode active material for lithium ion batteries according to claim 8, characterized in that: The reactants include SiH2ROH and SiH2RSH; Alternatively, the reactant comprises RSiCl3.

10. The method for preparing the negative electrode active material for lithium ion batteries according to claim 8, characterized in that: The organic solvent includes at least one of dimethyl sulfoxide, N,N-dimethylformamide, a sulfhydryl-containing compound, an alcohol solvent or an ether solvent.

11. The method for preparing a negative electrode active material for a lithium ion battery according to claim 8, characterized in that: The catalyst includes at least one of propylene glycol methyl ether acetate, N,N'-dicyclohexylcarbodiimide, aniline or potassium hydroxide.

12. The method for preparing the negative electrode active material for lithium ion batteries according to claim 7, characterized in that: The preparation of the organosiloxane polymer specifically comprises: The silicon precursor, the organic solvent and the catalyst are mixed uniformly, and the mixture is heated and pressurized to a second temperature and a first pressure under an inert gas atmosphere to react. After the reaction is completed, the mixture is cooled and pressurized to a third temperature and a second pressure under an inert gas atmosphere, and separated to obtain the organosiloxane polymer; Wherein, the second temperature is 110°C to 180°C, the first pressure is 1.0 atm to 3.0 atm; the reaction time at the second temperature and the first pressure is 70h to 100h; The third temperature is 22° C. to 28° C., and the second pressure is 0.9 atm to 1.1 atm.

13. The method for preparing a negative electrode active material for a lithium ion battery according to claim 12, characterized in that: The molar ratio of the silicon precursor, the organic solvent and the catalyst is 1:(12-20):(0.4-0.85).

14. The method for preparing a negative electrode active material for a lithium ion battery according to claim 12, characterized in that: The temperature increase rate is 1-5°C / h, and the pressure increase rate is 0.04-0.08atm / h.

15. The method for preparing a negative electrode active material for a lithium ion battery according to claim 12, characterized in that: The temperature reduction rate is 0.5-5°C / h, and the pressure reduction rate is 0.02-0.08atm / h.

16. The method for preparing a negative electrode active material for a lithium ion battery according to any one of claims 7 to 15, characterized in that: The organic siloxane polymer is used as a matrix material and an atomic layer deposition process is used to form a carbon coating layer on the surface of the organic siloxane polymer, specifically comprising: Introducing a carrier gas into an atomic layer deposition device, placing an organosiloxane polymer into the atomic layer deposition device, introducing a first gas-phase carbon source, and performing a first gas-phase deposition after heating to perform a first stage of carbon coating on the surface of the organosiloxane polymer; Then the temperature is lowered, and a second gas-phase carbon source is introduced, and the temperature is raised to perform a second gas-phase deposition, so as to perform a second stage of carbon coating on the surface of the organosiloxane polymer, and form a carbon coating layer on the surface of the organosiloxane polymer; Wherein, the heating temperature is 20°C to 40°C, and the heating time is 2h to 5h.

17. The method for preparing a negative electrode active material for a lithium ion battery according to claim 16, characterized in that: The cooling temperature is ≤20°C, and the cooling time is 3h to 6h.

18. The method for preparing a negative electrode active material for a lithium ion battery according to claim 16, characterized in that: The first gas-phase carbon source and the second gas-phase carbon source satisfy the following relationship: 2≤unsaturation of the first gas-phase carbon source≤unsaturation of the second gas-phase carbon source≤6; And / or, taking the amount of the organosiloxane polymer as 1 eq as a reference, the gas flow rates of the first gas-phase carbon source and the second gas-phase carbon source introduced satisfy the following relationship: 1eq≤the gas flow rate of the first gas-phase carbon source≤the gas flow rate of the second gas-phase carbon source≤4eq.

19. A battery comprising a negative electrode plate, characterized in that: The negative electrode plate comprises the negative electrode active material for a lithium ion battery according to any one of claims 1 to 6 or the negative electrode active material for a lithium ion battery prepared by the method according to any one of claims 7 to 18.

Citation Information

Patent Citations

  • Preparation method of negative composite material for lithium battery, negative electrode and lithium ion battery

    CN103872327A

  • Method for producing negative electrode active material for lithium ion secondary batteries

    CN109314235A