A high-performance modified PVC alloy and its preparation method and application

By adding ASA rubber powder and nanoclay with specific particle sizes into PVC materials, combined with hydrotalcite and thermal stabilizers, the problem of insufficient thermal stability and weather resistance of traditional PVC materials in photovoltaic cables is solved, and high-performance modification is achieved The high strength and weather resistance of PVC alloy are suitable for industries such as photovoltaic cables.

CN118307903BActive Publication Date: 2024-10-15ZHEJIANG YONGTONG NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410514952.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-26
Publication Date
2024-10-15
Estimated Expiration
2044-04-26

AI Technical Summary

Technical Problem

Due to poor thermal stability, low strength and insufficient weather resistance of traditional PVC materials in photovoltaic cables, they are prone to deformation, damage and brittleness in harsh environments, affecting the safety and reliability of photovoltaic equipment.

Method used

Using high-performance modified PVC alloy, by adding ASA rubber powder, hydrotalcite and nano-clay with low average rubber particle size, combined with a specific proportion of composite formula and heat stabilizer, the impact strength, thermal stability and weather resistance of the material are improved.

Benefits of technology

The impact strength, thermal stability and weather resistance of the modified PVC alloy are significantly improved, allowing it to exhibit the advantages of high strength, heat resistance and weather resistance in harsh environments, meeting the needs of photovoltaic cables.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004813065680000041
    Figure BDA0004813065680000041
  • Figure BDA0004813065680000051
    Figure BDA0004813065680000051
  • Figure BDA0004813065680000052
    Figure BDA0004813065680000052
Patent Text Reader

Abstract

The invention discloses a high-performance modified PVC alloy and a preparation method and application thereof, belonging to the technical field of modified plastics. The high-performance modified PVC alloy of the invention comprises the following components by weight: 100 parts of PVC resin, 15-30 parts of composite ASA rubber powder, 30-60 parts of plasticizer, 15-40 parts of toughener, 10-20 parts of hydrotalcite, 10-50 parts of nano clay, 1-2 parts of lubricant, 0.2-2 parts of heat stabilizer, the composite ASA rubber powder is obtained by melt extrusion of a first ASA rubber powder with an average rubber particle size of 80nm-150nm and a second ASA rubber powder with an average rubber particle size of 600-800nm, and the weight ratio of the hydrotalcite to the nano clay is 1: (2-5). The invention adds ASA rubber powder with a specific particle size combination and a specific proportion of hydrotalcite and nano clay to PVC, so that the PVC material has the advantages of high strength, heat resistance and good weather resistance, and can be applied to industries such as photovoltaic cables.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a high-performance modified PVC alloy and a preparation method and application thereof. Background Art

[0002] In recent years, in order to promote the utilization of solar energy resources and the development of the country's new energy industry, the photovoltaic industry has developed rapidly. Cables, as an important component of photovoltaic equipment, are directly related to the safety and reliability of solar photovoltaic power generation systems. Photovoltaic equipment is often used in harsh environmental conditions, such as high temperature, ultraviolet radiation, drastic climate change and chemical erosion; during installation and maintenance, cables may need to be routed on the sharp edges of roof structures and must withstand pressure, bending, tension, stretching and impact tests, which requires photovoltaic cables to have higher strength and weather resistance than traditional cables. Photovoltaic cables mostly use composite structure cables, which are mainly composed of copper strands, armor layers, and insulating layers or sheaths. Among them, the insulating layer or sheath is mostly made of polyvinyl chloride (PVC), which is insulating, corrosion-resistant and inexpensive. However, PVC materials have obvious disadvantages: first, they have poor thermal stability and are very easy to decompose. Unmodified PVC resins have no use value; second, they are brittle and have relatively low strength. During transportation and installation, they are prone to problems such as deformation, damage, and brittle cracks. At the same time, the addition of plasticizers in flexible PVC will also have a negative impact on the wear resistance and heat resistance of PVC materials, seriously affecting the operating safety of photovoltaic equipment, which greatly limits the application of PVC. Summary of the invention

[0003] In order to overcome the deficiencies of the above-mentioned prior art, the object of the present invention is to provide a high-performance modified PVC alloy having the characteristics of high strength, heat resistance, good weather resistance and the like.

[0004] Another object of the present invention is to provide a method for preparing a high-performance modified PVC alloy.

[0005] The invention is realized by the following technical scheme: a high-performance modified PVC alloy, which comprises the following components by weight: 100 parts of PVC resin, 15-30 parts of composite ASA rubber powder, 30-60 parts of plasticizer, 15-40 parts of toughening agent, 10-20 parts of hydrotalcite, 10-50 parts of nano clay, 1-2 parts of lubricant and 0.2-2 parts of heat stabilizer. The composite ASA rubber powder is obtained by melt extrusion of a first ASA rubber powder with an average rubber particle size of 80nm-150nm and a second ASA rubber powder with an average rubber particle size of 600-800nm, and the weight ratio of the hydrotalcite to the nano clay is 1:(2-5).

[0006] Preferably, the average degree of polymerization of the PVC resin is 1700-2500, and the average degree of polymerization of the PVC resin can be measured according to GB / T 5761-2018.

[0007] Preferably, the weight ratio of the first ASA rubber powder to the second ASA rubber powder is 1:(0.5-2), and further preferably, the weight ratio of the first ASA rubber powder to the second ASA rubber powder is 1:1.

[0008] Preferably, the weight ratio of the hydrotalcite to the nanoclay is 1:(3-4).

[0009] Preferably, the nanoclay is selected from one or more of montmorillonite, bentonite and kaolinite. More preferably, the nanoclay is selected from montmorillonite.

[0010] Preferably, the lubricant is selected from one or more of calcium stearate, magnesium stearate and polyethylene wax.

[0011] Preferably, the toughening agent is one or more selected from MBS and chlorinated polyethylene.

[0012] Preferably, the heat stabilizer is selected from organotin stabilizers; further preferably, the organotin stabilizer is selected from any one or more of methyltin mercaptan or maleic anhydride organotin.

[0013] The present invention also protects a method for preparing the above-mentioned high-performance modified PVC alloy, comprising the following steps:

[0014] PVC, plasticizer, heat stabilizer and lubricant are mixed evenly, heated to 80-110°C, and then mixed evenly with composite ASA rubber powder, toughening agent, hydrotalcite and organic clay, and granulated by extruder, and the temperature range of the extruder is 80-170°C.

[0015] The present invention also protects the application of the high-performance modified PVC alloy in photovoltaic cable materials.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] The present invention provides a high-performance modified PVC alloy. By adding ASA rubber powder with low average rubber particles and ASA rubber powder with high average rubber particle size to compound, the impact strength and toughness of the modified PVC alloy are improved, and the thermal stability of the material and its weather resistance can also be increased. Hydrotalcite and nanoclay are compounded in a certain proportion and applied to the modified PVC alloy, which can further improve the thermal stability, heat resistance and weather resistance of the modified PVC alloy, and the addition of nanoclay can improve the mechanical strength and toughness of the modified PVC alloy. The present invention adds ASA rubber powder with a specific particle size and a specific proportion of hydrotalcite and nanoclay to PVC, so that the PVC material has the advantages of high strength, heat resistance and good weather resistance, and can be applied to industries such as photovoltaic cables. DETAILED DESCRIPTION

[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] In the examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0020] The raw materials used in the embodiments and comparative examples are described as follows:

[0021] PVC resin 1: Xinjiang Tianye, TYH-2500, average degree of polymerization is 2500;

[0022] PVC resin 2: Formosa Plastics, PVC S-80, average degree of polymerization 1800;

[0023] PVC resin 3: Formosa Plastics, PVC S-75, average degree of polymerization 1450;

[0024] ASA rubber powder 1: Kumho Petrochemical, XC510A, average rubber particle size 100nm;

[0025] ASA rubber powder 2: Donghai Plastics, DH10, average rubber particle size is 600nm;

[0026] ASA rubber powder 3, Donghai Plastics, Q350, average rubber particle size is 800nm;

[0027] Plasticizer: dioctyl terephthalate, DOTP, Weilianda;

[0028] Toughener: MBS, B717, Dow;

[0029] Hydrotalcite: 99%, Lambovan;

[0030] Nanoclay 1: montmorillonite, DK-NF, Fenghong;

[0031] Nanoclay 2: bentonite, DK3, Fenghong;

[0032] Nanoclay 3: kaolin, T90, Fengtai New Materials;

[0033] Lubricant: polyethylene wax, PE520, Clariant;

[0034] Heat stabilizer: organic tin stabilizer, SW-977, Hubei Benxing;

[0035] Unless otherwise specified, the components and raw materials used in the embodiments and comparative examples of the present invention are all commercially available raw materials, and the components and raw materials used in each parallel experiment are all of the same kind.

[0036] Example 1-15 A high performance modified PVC alloy and its preparation method

[0037] Embodiment 1-15 provides a high-performance modified PVC alloy and a preparation method thereof. The weight formula thereof is shown in Table 1. The preparation method is as follows:

[0038] 1) Weigh the raw materials by weight;

[0039] 2) PVC, plasticizer, heat stabilizer and lubricant are mixed evenly, heated to 80-110°C, and then mixed evenly with composite ASA rubber powder, toughening agent, hydrotalcite and organic clay, and granulated by extruder, and the temperature range of the extruder is 80-170°C.

[0040] Table 1

[0041]

[0042]

[0043] Table 1

[0044] Example 10 Embodiment 11 Example 12 Example 13 Embodiment 14 Embodiment 15 PVC resin 1 100 100 100 100 100 100 ASA Rubber Powder 1 15 5 7 13 7.5 15 ASA Rubber Powder 2 5 15 13 7 7.5 15 Plasticizers 50 50 50 50 30 60 Toughening agent 20 20 20 20 15 40 Hydrotalcite 15 15 15 15 10 20 Nano clay 1 45 45 45 45 20 50 Lubricants 1 1 1 1 1 2 Heat Stabilizer 0.2 0.2 0.2 0.2 0.2 2

[0045] The preparation method of Comparative Examples 1-8 is the same as that of Examples 1-15, and the weight formula is shown in Table 2

[0046]

[0047]

[0048] The high performance modified PVC alloys prepared in Examples 1-15 and Comparative Examples 1-8 were subjected to the following performance tests, and the results are shown in Table 3.

[0049] 1. Impact strength: The products of the embodiments and comparative examples were subjected to an Izod notched impact test according to ISO 180-2000, with an A-notch;

[0050] 2. Heat deformation temperature: The products of the embodiments and comparative examples were tested based on ISO75-2-2013 standard, and the test pressure was 0.45 MPa;

[0051] 3. Impact strength retention rate after light aging: The products of the examples and comparative examples were subjected to a 1000-h xenon lamp aging test according to the ISO4892-22013 standard method, and then the performance retention rate of the cantilever beam notched impact test was tested according to the ISO 180-2000 standard;

[0052] 4. Impact strength retention after thermal aging: According to ISO 188-2011 standard, the products of the examples and comparative examples were subjected to thermal oxygen aging test at a temperature of 150° C. for 2000 h, and then the performance retention of the cantilever beam notched impact test was tested according to ISO 180-2000 standard.

[0053] Table 3

[0054]

[0055]

[0056] The present invention provides a high-performance modified PVC alloy, the impact strength of which is ≥20KJ / m 2 , heat deformation temperature ≥150℃, impact strength retention rate after light aging ≥78%, impact strength retention rate after heat aging ≥85%, meeting the use requirements of photovoltaic cables in harsh environments.

[0057] It can be seen from Examples 1, 10-13, and Comparative Examples 1-2 that by adding ASA rubber powder with low average rubber particles and compounding it with ASA rubber powder with high average rubber particle size, the impact strength of the modified PVC alloy is improved, and the thermal stability of the material and its weather resistance can also be increased. When the ratio of ASA rubber powder with low average rubber particles to ASA rubber powder with high average rubber particle size is preferably in the range of 1: (0.5-2), the improvement effect of its toughness, thermal stability and weather resistance is better.

[0058] It can be seen from Examples 1, 5-7, and Comparative Examples 3-4 that the application of hydrotalcite and nanoclay in a certain proportion in the modified PVC alloy can further improve the impact strength, thermal stability, heat resistance and weather resistance of the modified PVC alloy. When the preferred weight ratio of hydrotalcite and nanoclay is 1:(3-4), the improvement effect of toughness, thermal stability and weather resistance is better.

[0059] It can be seen from Examples 1-3 that when the average degree of polymerization of the PVC resin is selected to be 1700-2500, the improvement effect of its toughness, thermal stability and weather resistance is better.

[0060] It can be seen from Examples 1, 8 and 9 that when montmorillonite is selected as the nanoclay, the improvement effect of its toughness, thermal stability and weather resistance is better, which may be related to its layered structure.

[0061] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A high performance modified PVC alloy, characterized in that: The invention comprises the following components by weight: 100 parts of PVC resin, 15-30 parts of composite ASA rubber powder, 30-60 parts of plasticizer, 15-40 parts of toughening agent, 10-20 parts of hydrotalcite, 10-50 parts of nano clay, 1-2 parts of lubricant, and 0.2-2 parts of heat stabilizer. The composite ASA rubber powder is obtained by melt-extruding a first ASA rubber powder with an average rubber particle size of 100 nm and a second ASA rubber powder with an average rubber particle size of 600 nm, and the weight ratio of the first ASA rubber powder to the second ASA rubber powder is 1:1; the hydrotalcite is The weight ratio of the modified PVC alloy to the nanoclay is 1:(3-4); the nanoclay is selected from montmorillonite; the toughening agent is selected from MBS; the heat stabilizer is selected from organic tin stabilizers; the preparation method of the high-performance modified PVC alloy comprises the following steps: uniformly mixing PVC, plasticizer, hydrotalcite, organic clay and heat stabilizer, heating to 80-110°C and then uniformly mixing with composite ASA rubber powder, lubricant and toughening agent, granulating through an extruder, and the temperature range of the extruder is 80-170°C; the modified PVC alloy is used in photovoltaic cable materials.

2. The modified PVC alloy according to claim 1, characterized in that: The average polymerization degree of the PVC resin is 1700-2500.

3. The modified PVC alloy according to claim 1, characterized in that: The lubricant is selected from one or more of calcium stearate, magnesium stearate and polyethylene wax.

4. The modified PVC alloy according to claim 1, characterized in that: The plasticizer is selected from one or more of epoxy plasticizers, terephthalate plasticizers, cyclohexane dicarboxylate plasticizers or citrate plasticizers.

5. The modified PVC alloy according to claim 1, characterized in that: The organotin stabilizer is selected from any one or more of methyltin mercaptan or maleic anhydride organotin.