Oilfield anti-scaling and desulfurizing agent and preparation method thereof
By using a combination of polyamino compounds, modified activated carbon and other components to prepare an anti-scaling desulfurizer for oil fields, it solves the problems of clogging and poor desulfurization effect of existing desulfurizers, achieves efficient desulfurization and anti-scaling performance, and is suitable for oil fields technology and simplifies the preparation process.
Patent Information
- Application Number
- CN202410756639.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-13
AI Technical Summary
Existing oilfield desulfurizers can easily cause pipeline blockage during use, and the desulfurization effect is not ideal, making it difficult to achieve excellent desulfurization and anti-scaling properties at the same time.
Oilfield anti-scaling desulfurizers are prepared using a combination of polyamino compounds, modified activated carbon and inorganic salts through specific preparation methods, including modifying chitosan with methoxybenzaldehyde, grafting with acrylamide, and The diethylene triamine terminal amino group is hyperbranched, combined with modified activated carbon and inorganic salts, and added with a dispersant to form a desulfurizer with excellent desulfurization and anti-scaling properties.
It significantly improves the desulfurization effect and anti-scaling performance, avoids pipeline blockage, is suitable for oil field desulfurization processes, simplifies the preparation process, and is widely used in industrial production.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical desulfurization, in particular to an oilfield anti-scaling and desulfurizing agent and a preparation method thereof. Background Art
[0002] During oilfield development, hydrogen sulfide gas is produced due to the oxidation and decomposition of microorganisms and the high-temperature cracking process. Hydrogen sulfide is an irritating gas with strong toxicity. It is harmful to the human body and the environment and has a certain corrosive effect on equipment. Therefore, industrial desulfurizers are a powerful means to remove hydrogen sulfide. There are various types of desulfurizers on the market, including triazine desulfurizers and organic amine desulfurizers. These desulfurizers have certain good effects, but they will cause pipeline blockage to a certain extent, and the desulfurization effect will also be reduced. Producing a desulfurizer with excellent desulfurization and anti-scaling performance has a broader application prospect. Summary of the invention
[0003] 1. Technical issues to be resolved
[0004] In view of the deficiencies of the prior art, the present invention provides an oilfield anti-scaling and desulfurizing agent and a preparation method thereof, which has better desulfurization effect and anti-scaling ability.
[0005] (II) Technical solution
[0006] An oilfield anti-scaling and desulfurizing agent comprises the following components in percentage by mass:
[0007] 40~60% polyamino compound, 10~20% modified activated carbon, 5~10% inorganic salt, 1~5% synergist, 5~44% dispersant;
[0008] The preparation method of the polyamino compound is as follows:
[0009] (1) Add chitosan to a 10% by mass acetic acid solution, stir to dissolve, pass nitrogen, add p-methoxybenzaldehyde dropwise, heat under reflux for 20-30 h, and cool to room temperature to obtain modified chitosan;
[0010] (2) Dissolve acrylamide in water, heat the modified chitosan to 50-60°C, add the acrylamide aqueous solution, then add the initiator ammonium persulfate, heat to 80-90°C and react for 2-6 h, stop the reaction, cool to room temperature, and obtain modified chitosan grafted with acrylamide;
[0011] (3) Add diethylenetriamine to a flask, cool in an ice-water bath, pass nitrogen, slowly drop modified chitosan grafted acrylamide and methanol, react at room temperature for 2-6 h, transfer to a rotary evaporator in an eggplant-shaped flask, remove methanol under reduced pressure, heat to 130-150°C and continue to react under reduced pressure for 2-6 h, stop the reaction, and obtain amino-terminated hyperbranched modified chitosan grafted acrylamide, i.e., a polyamino compound;
[0012] The preparation method of the modified activated carbon is as follows:
[0013] (4) Grind the activated carbon through a 100-mesh sieve, boil it in deionized water for 10 to 30 min, filter it after cooling, repeat the operation three times, and dry it in a constant temperature drying oven to constant weight; soak the treated activated carbon in a mixed solution of sodium carbonate, sodium benzoate, and sodium acrylate for 10 to 30 h, then wash it with deionized water until it is neutral, and dry it at 100 to 120 °C for 6 to 12 h to obtain modified activated carbon;
[0014] The preparation method of the desulfurizing agent is as follows:
[0015] (5) Add the polyamino compound into a mixer and stir, add the modified activated carbon, stir evenly, add the inorganic salt and synergist, stir at 60-80°C for 30-60 min, cool to room temperature, add the dispersant, stir evenly, and obtain a desulfurizer;
[0016] The dispersant is one or more of ethanol, ethylene glycol, propylene glycol and methanol.
[0017] Preferably, in step (1), the weight ratio of chitosan to p-methoxybenzaldehyde is 1:1.2-2.
[0018] Preferably, in step (2), the weight ratio of acrylamide, modified chitosan, and initiator ammonium persulfate is 1:0.6-1.2:0.01-0.03.
[0019] Preferably, in step (3), the mass ratio of diethylenetriamine, modified chitosan grafted acrylamide, and methanol is 1:0.5-0.8:2-2.5.
[0020] Preferably, in step (4), the mass ratio of sodium carbonate, sodium benzoate and sodium acrylate is 1:0.3-0.6:0.6-0.8.
[0021] Preferably, the inorganic salt is one or more of aluminum oxide, zinc oxide, ferric chloride and ferric sulfate.
[0022] Preferably, the synergist is a desulfurization synergist.
[0023] 3. Beneficial technical effects
[0024] An oilfield anti-scaling and desulfurizing agent comprises: 40-60% of polyamino compounds, 10-20% of modified activated carbon, 5-10% of inorganic salts, 1-5% of synergist, and 5-44% of dispersant.
[0025] Chitosan is modified by p-methoxybenzaldehyde, grafted with acrylamide, and then hyperbranched with diethylenetriamine terminal amino groups to obtain polyamino compounds. Methoxy groups have electron-withdrawing properties, and polyamino compounds are alkaline, which can effectively reduce the concentration of hydrogen sulfide. Modified activated carbon can greatly improve the desulfurization effect of desulfurizers.
[0026] The invention has good desulfurization effect and anti-scaling performance, is suitable for oil field desulfurization technology, and has simple preparation process and is widely used in industrial production. DETAILED DESCRIPTION
[0027] Example 1
[0028] (1) Add 30 g of chitosan into 500 mL of 10% glacial acetic acid solution, stir to dissolve, pass nitrogen, add 30 mL of methoxybenzaldehyde dropwise, heat under reflux for 20 h, and cool to room temperature to obtain modified chitosan.
[0029] (2) Dissolve 100 g of acrylamide in 500 mL of water, heat the modified chitosan to 50 °C, add the acrylamide aqueous solution, and then add 1 g of initiator ammonium persulfate. Heat to 80 °C and react for 2 h. Stop the reaction and cool to room temperature to obtain modified chitosan grafted with acrylamide.
[0030] (3) Add 320 g of diethylenetriamine into a flask, cool in an ice-water bath, pass nitrogen, slowly dropwise add modified chitosan grafted acrylamide and 640 mL of methanol, react at room temperature for 2 h, transfer to an eggplant-shaped flask of a rotary evaporator, remove methanol under reduced pressure, raise the temperature to 130 °C and continue to react under reduced pressure for 2 h, stop the reaction, and obtain terminal amino hyperbranched modified chitosan grafted acrylamide, i.e., a polyamino compound.
[0031] (4) Grind 150 g of activated carbon and pass it through a 100-mesh sieve. Boil it in deionized water for 10 min, cool it and filter it. Repeat the operation three times and dry it in a constant temperature drying oven to constant weight. Add the treated activated carbon into 800 mL of a mixed solution of 30 g of sodium carbonate, 9 g of sodium benzoate and 18 g of sodium acrylate and soak it for 10 h. Then wash it with deionized water until it is neutral and dry it at 100 °C for 6 h to obtain modified activated carbon.
[0032] (5) Add 400 g of polyamino compound into a blender and stir, add 100 g of modified activated carbon and stir evenly, add 50 g of inorganic salt and 10 g of synergist, stir at 60 °C for 30 min, cool to room temperature, add 460 mL of dispersant and stir evenly to obtain a desulfurizer.
[0033] Example 2
[0034] (1) Add 60 g of chitosan into 1200 mL of 10% glacial acetic acid solution, stir to dissolve, pass nitrogen, add 120 mL of methoxybenzaldehyde dropwise, heat under reflux for 30 h, and cool to room temperature to obtain modified chitosan.
[0035] (2) Dissolve 150 g of acrylamide in 800 mL of water, heat the modified chitosan to 60 °C, add the acrylamide aqueous solution, and then add 4.5 g of initiator ammonium persulfate. Heat to 90 °C and react for 6 h. Stop the reaction and cool to room temperature to obtain modified chitosan grafted with acrylamide.
[0036] (3) Add 400 g of diethylenetriamine into a flask, cool in an ice-water bath, pass nitrogen, slowly drop modified chitosan grafted acrylamide and 1000 mL of methanol, react at room temperature for 6 h, transfer to an eggplant-shaped flask of a rotary evaporator, remove methanol under reduced pressure, raise the temperature to 150 °C and continue to react under reduced pressure for 6 h, stop the reaction, and obtain terminal amino hyperbranched modified chitosan grafted acrylamide, i.e., polyamino compound.
[0037] (4) Crush 300 g of activated carbon and pass it through a 100-mesh sieve. Boil it in deionized water for 30 min, cool it and filter it. Repeat the operation three times and dry it in a constant temperature drying oven to constant weight. Add the treated activated carbon into 1500 mL of a mixed solution of 60 g of sodium carbonate, 36 g of sodium benzoate and 48 g of sodium acrylate and soak it for 30 h. Then wash it with deionized water until it is neutral and dry it at 100-120 °C for 6-12 h to obtain modified activated carbon.
[0038] (5) Add 600 g of polyamino compound into a blender and stir, add 200 g of modified activated carbon and stir evenly, add 100 g of inorganic salt and 50 g of synergist, stir at 80 °C for 60 min, cool to room temperature, add 60 mL of dispersant and stir evenly to obtain a desulfurizer.
[0039] Example 3
[0040] (1) Add 40 g of chitosan into 600 mL of 10% glacial acetic acid solution, stir to dissolve, pass nitrogen, add 50 mL of methoxybenzaldehyde dropwise, heat under reflux for 22 h, and cool to room temperature to obtain modified chitosan.
[0041] (2) Dissolve 120 g of acrylamide in 600 mL of water, heat the modified chitosan to 55 °C, add the acrylamide aqueous solution, and then add 2 g of initiator ammonium persulfate. Heat the temperature to 82 °C and react for 3 h. Stop the reaction and cool to room temperature to obtain modified chitosan grafted with acrylamide.
[0042] (3) Add 350 g of diethylenetriamine into a flask, cool in an ice-water bath, pass nitrogen, slowly dropwise add modified chitosan grafted acrylamide and 700 mL of methanol, react at room temperature for 3 h, transfer to an eggplant-shaped flask of a rotary evaporator, remove methanol under reduced pressure, raise the temperature to 140 °C and continue to react under reduced pressure for 3 h, stop the reaction, and obtain terminal amino hyperbranched modified chitosan grafted acrylamide, i.e., a polyamino compound.
[0043] (4) Grind 180 g of activated carbon and pass it through a 100-mesh sieve. Boil it in deionized water for 20 min, cool it and filter it. Repeat the operation three times and dry it in a constant temperature drying oven to constant weight. Add the treated activated carbon into 1000 mL of a mixed solution of 40 g of sodium carbonate, 15 g of sodium benzoate and 20 g of sodium acrylate and soak it for 12 h. Then wash it with deionized water until it is neutral and dry it at 110 °C for 8 h to obtain modified activated carbon.
[0044] (5) Add 450 g of polyamino compound into a blender and stir, add 120 g of modified activated carbon and stir evenly, add 60 g of inorganic salt and 20 g of synergist, stir at 66 °C for 40 min, cool to room temperature, add 40 mL of dispersant and stir evenly to obtain a desulfurizer.
[0045] Example 4
[0046] (1) Add 50 g of chitosan into 1000 mL of 10% glacial acetic acid solution, stir to dissolve, pass nitrogen, add 60 mL of methoxybenzaldehyde dropwise, heat under reflux for 25 h, and cool to room temperature to obtain modified chitosan.
[0047] (2) Dissolve 140 g of acrylamide in 700 mL of water, heat the modified chitosan to 55 °C, add the acrylamide aqueous solution, and then add 3 g of initiator ammonium persulfate. Heat to 90 °C and react for 4 h. Stop the reaction and cool to room temperature to obtain modified chitosan grafted with acrylamide.
[0048] (3) Add 360 g of diethylenetriamine into a flask, cool in an ice-water bath, pass nitrogen, slowly dropwise add modified chitosan grafted acrylamide and 900 mL of methanol, react at room temperature for 5 h, transfer to an eggplant-shaped flask of a rotary evaporator, remove methanol under reduced pressure, raise the temperature to 150 °C and continue to react under reduced pressure for 5 h, stop the reaction, and obtain terminal amino hyperbranched modified chitosan grafted acrylamide, i.e., a polyamino compound.
[0049] (4) Grind 200 g of activated carbon and pass it through a 100-mesh sieve, boil it in deionized water for 20 min, filter it after cooling, repeat the operation three times, and dry it in a constant temperature drying oven to constant weight; add the treated activated carbon into 1200 mL of a mixed solution of 50 g of sodium carbonate, 20 g of sodium benzoate, and 30 g of sodium acrylate and soak it for 20 h, then wash it with deionized water until it is neutral, and dry it at 120 °C for 10 h to obtain modified activated carbon.
[0050] (5) Add 520 g of polyamino compound into a blender and stir, add 180 g of modified activated carbon and stir evenly, add 80 g of inorganic salt and 30 g of synergist, stir at 70 °C for 50 min, cool to room temperature, add 25 mL of dispersant and stir evenly to obtain a desulfurizer.
[0051] Example 5
[0052] (1) Add 50 g of chitosan into 1200 mL of 10% glacial acetic acid solution, stir to dissolve, pass nitrogen, add 100 mL of methoxybenzaldehyde dropwise, heat under reflux for 24 h, and cool to room temperature to obtain modified chitosan.
[0053] (2) Dissolve 140 g of acrylamide in 600 mL of water, heat the modified chitosan to 60 °C, add the acrylamide aqueous solution, and then add 4 g of initiator ammonium persulfate. Heat to 90 °C and react for 5 h. Stop the reaction and cool to room temperature to obtain modified chitosan grafted with acrylamide.
[0054] (3) Add 380 g of diethylenetriamine into a flask, cool in an ice-water bath, pass nitrogen, slowly dropwise add modified chitosan grafted acrylamide and 900 mL of methanol, react at room temperature for 5 h, transfer to an eggplant-shaped flask of a rotary evaporator, remove methanol under reduced pressure, raise the temperature to 150 °C and continue to react under reduced pressure for 5 h, stop the reaction, and obtain terminal amino hyperbranched modified chitosan grafted acrylamide, i.e., a polyamino compound.
[0055] (4) Grind 250 g of activated carbon and pass it through a 100-mesh sieve, boil it in deionized water for 20 min, filter it after cooling, repeat the operation three times, and dry it in a constant temperature drying oven to constant weight; add the treated activated carbon into 1200 mL of a mixed solution of 60 g of sodium carbonate, 30 g of sodium benzoate, and 40 g of sodium acrylate and soak it for 20 h, then wash it with deionized water until it is neutral, and dry it at 100 °C for 10 h to obtain modified activated carbon.
[0056] (5) Add 600 g of polyamino compound into a blender and stir, add 100 g of modified activated carbon and stir evenly, add 80 g of inorganic salt and 40 g of synergist, stir at 80 °C for 50 min, cool to room temperature, add 26 mL of dispersant and stir evenly to obtain a desulfurizer.
[0057] Comparative Example 1: Commercially available triazine desulfurizer.
[0058] Desulfurization test:
[0059] Refer to ASTM D4810-88 (1999) "Standard Method for Determination of Hydrogen Sulfide Content in Natural Gas Using Colorimetric Detector Tube Method".
[0060] The desulfurization rate is used to evaluate the desulfurization performance of the desulfurizer. The higher the desulfurization rate, the better the desulfurization performance. The desulfurization rate refers to the percentage of the reduction in hydrogen sulfide content before and after the desulfurizer is added to the water sample. The desulfurization rate is calculated as follows:
[0061] X=[(C0-C) / C0] ×100%
[0062] Where:
[0063] X—desulfurization rate;
[0064] C0—hydrogen sulfide content measured before adding desulfurizer, ppm;
[0065] C—Hydrogen sulfide content measured after adding desulfurizer, ppm.
[0066] Table 1 Test results
[0067] Anti-scaling performance test:
[0068] Refer to SY / T5673-1993 Oilfield Antiscalant Performance Evaluation Method. According to the experimental conditions, take the corresponding 100 mL test medium and add it to the stoppered colorimetric tube. The desulfurizer filling concentration is 200 mg / L. Heat it to the test temperature of 55°C and keep it constant for 48 hours. After the temperature cools down, observe the scaling of the medium in the colorimetric tube. If scaling occurs, shake the medium and filter it, and perform a titration experiment. The titration experiment refers to GB7476-87 "Determination of calcium content in water - EDTA titration method".
[0069] The performance of anti-scaling agent is characterized by anti-scaling rate. The larger the percentage value, the better the anti-scaling performance. The anti-scaling rate E is calculated as follows:
[0070] E = [(M2-M1) / (M0-M1)] × 100%
[0071] Where:
[0072] M2—Calcium ion concentration in the produced liquid after adding the reagent;
[0073] M1—Calcium ion concentration in the produced fluid without adding reagents;
[0074] M0—initial calcium ion concentration in the produced fluid.
[0075] Table 2 Test results
[0076] It can be seen from Table 1 and Table 2 that Examples 1 to 5 have better desulfurization effect and better anti-scaling ability.
[0077] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
[0078] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An oilfield anti-scaling and desulfurizing agent, characterized in that: The desulfurizing agent comprises the following components in percentage by weight: 40~60% polyamino compound, 10~20% modified activated carbon, 5~10% inorganic salt, 1~5% synergist, 5~44% dispersant; The preparation method of the polyamino compound is as follows: (1) Add chitosan to a 10% by mass acetic acid solution, stir to dissolve, pass nitrogen, add p-methoxybenzaldehyde dropwise, heat under reflux for 20-30 h, and cool to room temperature to obtain modified chitosan; (2) Dissolve acrylamide in water, heat the modified chitosan to 50-60°C, add the acrylamide aqueous solution, then add the initiator ammonium persulfate, heat to 80-90°C and react for 2-6 h, stop the reaction, cool to room temperature, and obtain modified chitosan grafted with acrylamide; (3) Add diethylenetriamine to a flask, cool in an ice-water bath, pass nitrogen, slowly drop modified chitosan grafted acrylamide and methanol, react at room temperature for 2-6 h, transfer to a rotary evaporator in an eggplant-shaped flask, remove methanol under reduced pressure, heat to 130-150°C and continue to react under reduced pressure for 2-6 h, stop the reaction, and obtain amino-terminated hyperbranched modified chitosan grafted acrylamide, i.e., a polyamino compound; The preparation method of the modified activated carbon is as follows: (4) Grind the activated carbon through a 100-mesh sieve, boil it in deionized water for 10 to 30 min, filter it after cooling, repeat the operation three times, and dry it in a constant temperature drying oven to constant weight; soak the treated activated carbon in a mixed solution of sodium carbonate, sodium benzoate, and sodium acrylate for 10 to 30 h, then wash it with deionized water until it is neutral, and dry it at 100 to 120 °C for 6 to 12 h to obtain modified activated carbon; The preparation method of the desulfurizing agent is as follows: (5) Add the polyamino compound into a mixer and stir, add the modified activated carbon, stir evenly, add the inorganic salt and synergist, stir at 60-80°C for 30-60 min, cool to room temperature, add the dispersant, stir evenly, and obtain a desulfurizer; The dispersant is one or more of ethanol, ethylene glycol, propylene glycol, and methanol; In step (1), the weight ratio of chitosan to p-anisaldehyde is 1:1.2-2; The inorganic salt is one or more of aluminum oxide, zinc oxide, ferric chloride and ferric sulfate.
2. The oilfield anti-scaling and desulfurizing agent according to claim 1, characterized in that: In step (2), the weight ratio of acrylamide, modified chitosan and initiator ammonium persulfate is 1:0.6~1.2:0.01~0.
03.
3. The oilfield anti-scaling and desulfurizing agent according to claim 1, characterized in that: In step (3), the mass ratio of diethylenetriamine, modified chitosan grafted acrylamide and methanol is 1:0.5~0.8:2~2.
5.
4. The oilfield anti-scaling and desulfurizing agent according to claim 1, characterized in that: In step (4), the mass ratio of sodium carbonate, sodium benzoate and sodium acrylate is 1:0.3~0.6:0.6~0.
8.
5. The oilfield anti-scaling and desulfurizing agent according to claim 1, characterized in that: The synergist is a desulfurization synergist.