A wide temperature range electrolyte and its preparation method and application
By using lithium salt/amide compound deep eutectic solvents and additives in lithium-ion batteries to form a wide temperature range electrolyte, the problem of unsatisfactory performance of lithium-ion batteries in high and low temperature environments is solved, and the battery can operate in a wider temperature range. Efficient operation within the system expands the scope of application.
Patent Information
- Application Number
- CN202410725650.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-06
AI Technical Summary
The performance of existing lithium-ion batteries in high and low temperature environments is not ideal, mainly due to differences in the stability of lithium salts and differences in compatibility between lithium salts and solvents, resulting in insufficient wide-temperature performance of the electrolyte, which limits the application of lithium-ion batteries. scope.
Design a lithium salt/amide compound deep eutectic solvent, and add crown ether compounds, carbonate compounds and 1,2-dichloroethane as additives to form a wide temperature range electrolyte. The coordination reaction increases the dissociation degree and conductivity of lithium ions, reduces the viscosity, and improves the thermal stability and low-temperature conductivity of the electrolyte.
It enables lithium-ion batteries to maintain good electrochemical performance in a wider temperature range, improves the high and low temperature performance of the battery, broadens the application range of lithium-ion batteries, and reduces safety risks and costs.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery materials, and specifically discloses a wide temperature range electrolyte and a preparation method and application thereof. Background Art
[0002] Since its commercialization, lithium-ion batteries have become the mainstream power source for consumer electronics with their advantages of high energy density, high power density, long cycle life, low self-discharge rate, light weight and portability, and no memory effect. At present, the application scope of lithium-ion batteries has gradually expanded from consumer electronics to electric vehicles, large-scale clean energy access, national defense security and special applications, and is and will continue to make important contributions to the sustainable development of social economy. As the scope of application gradually expands, the requirements for lithium-ion batteries also increase. The optimal operating temperature of lithium-ion batteries is 10-30℃. Too high or too low temperatures will affect the performance of lithium-ion batteries and even cause safety problems. However, such a narrow operating temperature greatly limits the application of lithium-ion batteries. Therefore, how to prepare wide-temperature lithium-ion batteries has become an urgent problem to be solved in the battery field.
[0003] In recent years, due to the limited types of positive and negative electrode materials that can be applied to lithium-ion batteries, it is difficult to improve the wide temperature performance of the battery by optimizing the positive and negative electrode materials, so the expansion of the wide temperature performance of lithium-ion batteries is mainly focused on the optimization of the electrolyte. As for the optimization of wide temperature range electrolytes, the existing technology mainly optimizes the composition of the electrolyte by selecting suitable lithium salts, solvents or additives, and improves the thermal stability and low-temperature conductivity of the electrolyte, thereby obtaining a wide temperature range lithium-ion battery. However, the selection of electrolyte components has a great influence on the stability of the electrolyte, especially the difference in the stability of lithium salts and the difference in the compatibility of lithium salts and solvents, which leads to the performance of lithium-ion batteries in high and low temperature environments not meeting the ideal expectations. This has also become a new problem in the development of wide temperature range electrolytes.
[0004] Based on this, developing an electrolyte with a wide temperature range is of great significance to the development of lithium-ion batteries. Summary of the invention
[0005] In view of the problem in the prior art that the selection of wide temperature range electrolyte components affects the stability of the electrolyte, especially the difference in the stability of lithium salts and the difference in the compatibility of lithium salts and solvents, which directly leads to the unsatisfactory performance of lithium-ion batteries in high and low temperature environments, the present invention provides a wide temperature range electrolyte and its preparation method and application. The present invention designs a deep eutectic solvent, which uses lithium salts and amide compounds as raw materials and utilizes the strong interaction between the two to prepare the deep eutectic solvent; additives are added thereto to reduce the viscosity of the deep eutectic solvent, thereby improving the conductivity of the deep eutectic solvent, thereby achieving the purpose of improving the lithium ion conductivity.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] A first aspect of the present invention provides a wide temperature range electrolyte, wherein the wide temperature range electrolyte comprises a lithium salt / amide compound deep eutectic solvent and an additive.
[0008] Preferably, the amide compound comprises a first component and a second component, wherein the second component is N-dimethylacetamide.
[0009] Preferably, the additive comprises the following components in percentage by weight: 30%-50% of a crown ether compound, 30%-50% of a carbonate compound and 10%-25% of 1,2-dichloroethane.
[0010] Compared with the prior art, the present invention designs a lithium salt / amide compound deep eutectic solvent as the main component of a wide temperature range electrolyte. The present invention uses lithium ions as Lewis acids and amide compounds as Lewis bases, and utilizes Lewis acid-base interactions to form deep eutectic solvents. Among them, N-dimethylacetamide in amide compounds can interact with lithium ions through lithium-oxygen bonds, effectively increasing the solubility of lithium salts; and, the carbonyl groups in amide compounds coordinate with lithium ions to obtain lithium-nitrogen complexes, further promoting the dissociation of lithium ions in lithium salts and improving ionic conductivity. The lithium salt / amide compound deep eutectic solvent provided by the present invention has good thermal stability and chemical stability, good flame retardancy, low vapor pressure and excellent solubility, and has low safety risks under high temperature conditions; moreover, the preparation process of the lithium salt / amide compound deep eutectic solvent is simple, low cost and environmentally friendly. However, the inventors have found that the lithium salt / amide compound deep eutectic solvent has high viscosity and unsatisfactory ionic conductivity, which leads to poor performance of lithium-ion batteries under low temperature conditions. It is still difficult to meet the requirements of a wide temperature range by using only this lithium salt / amide compound deep eutectic solvent as the electrolyte.
[0011] Based on this, the present invention has designed an additive with crown ether compounds, carbonate compounds and 1,2-dichloroethane as raw materials, which is mixed with the lithium salt / amide compound deep eutectic solvent to prepare a wide temperature range electrolyte. Among them, the crown ether compound can improve the mechanical strength of the lithium deposition layer, effectively prevent the growth of lithium dendrites, thereby avoiding the problem of lithium dendrites piercing the diaphragm and causing the performance of the lithium ion battery to decrease, and effectively improve the cycle performance of the lithium ion battery at low temperature; and the carbonate compound can effectively adjust the structure and composition of the interface SEI film, promote its transformation to a multilayer structure, promote uniform lithium deposition, inhibit the growth of lithium dendrites, and thus improve the low temperature performance of the lithium battery; 1,2-dichloroethane can effectively reduce the viscosity of the deep eutectic solvent, so that it can maintain a low viscosity state at low temperatures, improve the low temperature conductivity of the electrolyte, and further improve the ionic conductivity of the electrolyte. By utilizing the synergistic effect of the three components, the purpose of reducing the viscosity of the deep eutectic solvent of lithium salt / amide compounds and improving the ionic conductivity of the electrolyte is achieved, so that the obtained electrolyte maintains good electrochemical properties regardless of low or high temperature conditions. The technical solution provided by the present invention effectively solves the problem in the prior art that the selection of wide temperature range electrolyte components affects the stability of the electrolyte, especially the difference in the stability of lithium salts and the difference in the compatibility of lithium salts and solvents directly lead to the unsatisfactory performance of lithium-ion batteries in high and low temperature environments, and provides a theoretical basis for the use of lithium-ion batteries in a wider temperature range.
[0012] Preferably, the first component is any one of 2-nitrobenzenesulfonamide, 2,2-dibromo-3-nitrilopropionamide, 5-amino-2-methylbenzenesulfonamide, caprolactam, 4-(2-aminoethyl)benzenesulfonamide or 4-chlorothiobenzamide.
[0013] Preferably, the mass ratio of the first component to the second component is 1-2:1-5.
[0014] Preferably, the molar ratio of the lithium salt to the first component in the amide compound is 1:1-1:5.
[0015] Further preferably, the molar ratio of the lithium salt to the first component in the amide compound is 1:1-1:2.
[0016] Preferably, the mass ratio of the additive to the lithium salt / amide compound deep eutectic solvent is 0.5:100-5:100.
[0017] Preferably, the lithium salt is any one of lithium difluorooxalate borate or lithium difluorosulfate borate.
[0018] Compared with lithium tetrafluoroborate or lithium hexafluoroborate commonly used in the prior art, lithium difluorooxalate borate and lithium difluorosulfate borate have better rate performance and cycle performance, and both can form a more stable SEI film on the graphite anode, improving the high temperature stability of lithium-ion batteries. More importantly, under high temperature conditions, lithium difluorooxalate borate or lithium difluorosulfate borate is not easy to decompose with trace amounts of water that may be produced, causing damage to the internal structure of the battery and thus reducing the service life of the lithium-ion battery.
[0019] Preferably, the crown ether compound is any one of 12-crown-4, 18-crown-6 or 15-crown-5.
[0020] The present invention adopts aliphatic crown ethers to effectively improve the compatibility of various components in the lithium ion battery electrolyte, effectively improve the lithium dendrite problem, and thus improve the interface stability and low temperature performance of the electrolyte.
[0021] Preferably, the carbonate compound is any one or both of fluoroethylene carbonate and fluoroethyl methyl carbonate.
[0022] The present invention adopts fluoroethylene carbonate or fluoroethyl methyl carbonate as carbonate compounds, utilizes fluorine substitution to increase the oxidation potential of carbonate, improves the thermal stability of carbonate, and thus further improves the thermal stability of electrode liquid.
[0023] Preferably, the preparation method of the lithium salt / amide compound deep eutectic solvent comprises the following steps: in a dry, low-oxygen environment, mixing the lithium salt and the amide compound evenly, stirring at 60°C-70°C until the solution is clear and transparent, to obtain the lithium salt / amide compound deep eutectic solvent.
[0024] Further preferably, the water content and oxygen content of the dry, low-oxygen environment are both ≤ 0.1 ppm.
[0025] A second aspect of the present invention provides a method for preparing a wide temperature range electrolyte, comprising the following steps: uniformly mixing the lithium salt / amide compound deep eutectic solvent and additives to obtain the wide temperature range electrolyte.
[0026] A third aspect of the present invention provides an application of the wide temperature range electrolyte in a lithium ion battery.
[0027] In summary, the present invention provides a wide temperature range electrolyte, a preparation method thereof, and an application thereof in lithium ion batteries. The present invention uses lithium salts and amide compounds as basic raw materials to prepare a deep eutectic solvent, and further uses additives to prepare the wide temperature range electrolyte. The wide temperature range electrolyte has good high and low temperature performance, and the lithium ion battery prepared using the wide temperature range electrolyte has good electrochemical properties at different temperatures. The present invention effectively solves the problem in the prior art that the selection of wide temperature range electrolyte components affects the stability of the electrolyte, especially the difference in the stability of lithium salts and the difference in the compatibility of lithium salts with solvents, which directly leads to the unsatisfactory performance of lithium ion batteries in high and low temperature environments. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] This embodiment provides a method for preparing a wide temperature range electrolyte, which specifically includes the following contents.
[0031] Step 1: In an argon glove box with a water content and an oxygen content of 0.1 ppm, 14.38 g of lithium difluorooxalatoborate, 40.45 g of 2-nitrobenzenesulfonamide and 100 g of N-dimethylacetamide were mixed evenly, and stirred at 65° C. until the solution became clear and transparent to obtain a lithium salt / amide compound deep eutectic solvent;
[0032] Step 2: Add 5 g of additive to the lithium salt / amide compound deep eutectic solvent and mix well to obtain the wide temperature range electrolyte.
[0033] The additive comprises the following components in percentage by weight: 40% of 12-crown ether-4, 50% of fluoroethylene carbonate and 10% of 1,2-dichloroethane.
[0034] Example 2
[0035] This embodiment provides a method for preparing a wide temperature range electrolyte, which specifically includes the following contents.
[0036] Step 1: In an argon glove box with a water content and an oxygen content of 0.1 ppm, 14.38 g of lithium difluorooxalatoborate, 48.37 g of 2,2-dibromo-3-nitrilopropionamide and 150 g of N-dimethylacetamide were mixed evenly, and stirred at 65° C. until the solution was clear and transparent to obtain a lithium salt / amide compound deep eutectic solvent;
[0037] Step 2: Add 6.36 g of additive to the lithium salt / amide compound deep eutectic solvent and mix well to obtain the wide temperature range electrolyte.
[0038] The additive comprises the following components in percentage by weight: 40% of 15-crown ether-5, 50% of fluoroethylene carbonate and 10% of 1,2-dichloroethane.
[0039] Example 3
[0040] This embodiment provides a method for preparing a wide temperature range electrolyte, which specifically includes the following contents.
[0041] Step 1: In an argon glove box with a water content and an oxygen content of 0.1 ppm, 14.38 g of lithium difluorooxalatoborate, 46.73 g of 5-amino-2-methylbenzenesulfonamide and 130 g of N-dimethylacetamide were mixed evenly, and stirred at 70° C. until the solution was clear and transparent to obtain a lithium salt / amide compound deep eutectic solvent;
[0042] Step 2: Add 7.2 g of additive to the lithium salt / amide compound deep eutectic solvent and mix well to obtain the wide temperature range electrolyte.
[0043] The additive includes the following components in percentage by weight: 40% of 18-crown ether-6, 45% of ethyl methyl fluorocarbonate and 15% of 1,2-dichloroethane.
[0044] Example 4
[0045] This embodiment provides a method for preparing a wide temperature range electrolyte, which specifically includes the following contents.
[0046] Step 1: In an argon glove box with a water content and an oxygen content of 0.1 ppm, 14.38 g of lithium difluorooxalatoborate, 47.46 g of caprolactam and 160 g of N-dimethylacetamide were mixed evenly, and stirred at 60° C. until the solution was clear and transparent to obtain a lithium salt / amide compound deep eutectic solvent;
[0047] Step 2: Add 3.8 g of additive to the lithium salt / amide compound deep eutectic solvent and mix well to obtain the wide temperature range electrolyte.
[0048] The additive includes the following components in percentage by weight: 50% of 15-crown ether-5, 30% of ethyl methyl fluorocarbonate and 20% of 1,2-dichloroethane.
[0049] Example 5
[0050] This embodiment provides a method for preparing a wide temperature range electrolyte, which specifically includes the following contents.
[0051] Step 1: In an argon glove box with a water content and an oxygen content of 0.1 ppm, 14.38 g of lithium difluorooxalatoborate, 42.7 g of 4-(2-aminoethyl)benzenesulfonamide and 142 g of N-dimethylacetamide were mixed evenly, and stirred at 60° C. until the solution became clear and transparent to obtain a lithium salt / amide compound deep eutectic solvent;
[0052] Step 2: Add 8 g of additives to the lithium salt / amide compound deep eutectic solvent and mix well to obtain the wide temperature range electrolyte.
[0053] The additive includes the following components in percentage by weight: 35% of 12-crown ether-4, 50% of ethyl methyl fluorocarbonate and 15% of 1,2-dichloroethane.
[0054] Example 6
[0055] This embodiment provides a method for preparing a wide temperature range electrolyte, which specifically includes the following contents.
[0056] Step 1: In an argon glove box with a water content and an oxygen content of 0.1 ppm, 14.38 g of lithium difluorooxalatoborate, 35.68 g of 4-chlorothiobenzamide and 120 g of N-dimethylacetamide were mixed evenly, and stirred at 70° C. until the solution was clear and transparent to obtain a lithium salt / amide compound deep eutectic solvent;
[0057] Step 2: Add 4.75 g of additive to the lithium salt / amide compound deep eutectic solvent and mix well to obtain the wide temperature range electrolyte.
[0058] The additive comprises the following components in percentage by weight: 35% of 18-crown ether-6, 45% of fluoroethylene carbonate and 20% of 1,2-dichloroethane.
[0059] Example 7
[0060] This embodiment provides a method for preparing a wide temperature range electrolyte, which specifically includes the following contents.
[0061] Step 1: In an argon glove box with a water content and an oxygen content of 0.1 ppm, 14.38 g of lithium difluorooxalate borate, 72.84 g of 2-nitrobenzenesulfonamide and 145 g of N-dimethylacetamide were mixed evenly, and stirred at 70° C. until the solution became clear and transparent to obtain a lithium salt / amide compound deep eutectic solvent;
[0062] Step 2: Add 8.76 g of additive to the lithium salt / amide compound deep eutectic solvent and mix well to obtain the wide temperature range electrolyte.
[0063] The additive includes the following components in percentage by weight: 45% of 15-crown ether-5, 35% of fluoroethylene carbonate and 20% of 1,2-dichloroethane.
[0064] Comparative Example 1
[0065] This comparative example provides an electrolyte, which is different from Example 1 in that the additive is 1,2-dichloroethane, and specifically includes the following contents.
[0066] Step 1: In an argon glove box with a water content and an oxygen content of 0.1 ppm, 14.38 g of lithium difluorooxalatoborate, 40.45 g of 2-nitrobenzenesulfonamide and 100 g of N-dimethylacetamide were mixed evenly, and stirred at 65° C. until the solution became clear and transparent to obtain a lithium salt / amide compound deep eutectic solvent;
[0067] Step 2: Add 5 g of 1,2-dichloroethane to the lithium salt / amide compound deep eutectic solvent and mix well to obtain the electrolyte.
[0068] Comparative Example 2
[0069] This comparative example provides an electrolyte, which differs from Example 1 in that no additives are added, and specifically includes the following contents.
[0070] In an argon glove box with a water content and an oxygen content of 0.1 ppm, 14.38 g of lithium difluorooxalatoborate, 40.45 g of 2-nitrobenzenesulfonamide and 100 g of N-dimethylacetamide were mixed uniformly and stirred at 65° C. until the solution was clear and transparent to obtain an electrolyte.
[0071] Comparative Example 3
[0072] This comparative example provides an electrolyte, which is different from Example 1 in that the amide compound is replaced by an equimolar amount of propenyl-1,3-sultone, and specifically includes the following contents.
[0073] Step 1: In an argon glove box with a water content and an oxygen content of 0.1 ppm, 14.38 g of lithium difluorooxalatoborate, 24.02 g of propenyl-1,3-sultone and 100 g of N-dimethylacetamide were mixed evenly, and stirred at 65° C. until the solution was clear and transparent to obtain a lithium salt / amide compound deep eutectic solvent;
[0074] Step 2: Add 5 g of additive to the lithium salt / amide compound deep eutectic solvent and mix well to obtain the wide temperature range electrolyte.
[0075] The additive comprises the following components in percentage by weight: 40% of 12-crown ether-4, 50% of fluoroethylene carbonate and 10% of 1,2-dichloroethane.
[0076] In order to reflect the technical effect of the present invention, the present invention applies the composite positive electrode materials obtained in Example 1 and Comparative Examples 1-3 to lithium-ion batteries, and tests the electrochemical properties of the obtained lithium-ion batteries under a wide temperature range. As shown in the test examples, the technical effects of Examples 2-7 are equivalent to those of Example 1.
[0077] Test example
[0078] This test example provides a lithium-ion battery (60mm×80mm soft-pack battery, voltage 4.0V), the positive electrode sheet material is lithium iron phosphate, the negative electrode sheet material is graphite, cellgard2500 is used as the battery separator, and the materials obtained in each embodiment and comparative example are electrolytes.
[0079] The parameters for low-temperature charge and discharge are as follows: the battery is tested in the blue battery test system, the test voltage is 2.7V-4.2V, and the rate performance test conditions are as follows: after charging at 0.5C, it is placed at -60℃, -50℃, -40℃, -30℃, -20℃, -10℃, 0℃, 10℃, 20℃, 30℃, 40℃, 50℃, 60℃ and 70℃ for 4h, discharged, and cycled for 400 weeks. The discharge capacity of the obtained lithium-ion battery at low temperature and the capacity retention rate of the cycle operation are tested, and the results are shown in Table 1.
[0080] Table 1 Lithium-ion battery performance test results
[0081]
[0082] It can be seen from Table 1 that the lithium ion battery prepared by using the wide temperature range electrolyte provided in Example 1 of the present invention has better high and low temperature performance. At -60°C, the discharge capacity is still as high as 1643 mAh, and even after 400 cycles, the capacity retention rate is as high as 62.3%; at 70°C, the discharge capacity can still reach 1863 mAh, and even after 400 cycles, the capacity retention rate is as high as 64.1%; it can be seen that the wide temperature range electrolyte provided by the present invention can effectively improve the electrochemical performance of lithium ion batteries in high and low temperature environments, and broaden the application scope of lithium ion batteries.
[0083] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A wide temperature range electrolyte, characterized in that: The wide temperature range electrolyte comprises a lithium salt / amide compound deep eutectic solvent and an additive; The amide compound comprises a first component and a second component, wherein the second component is N-dimethylacetamide; The additive comprises the following components in percentage by weight: 30%-50% of a crown ether compound, 30%-50% of a carbonate compound and 10%-25% of 1,2-dichloroethane; The first component is any one of 2-nitrobenzenesulfonamide, 2,2-dibromo-3-nitrilopropionamide, 5-amino-2-methylbenzenesulfonamide, caprolactam, 4-(2-aminoethyl)benzenesulfonamide or 4-chlorothiobenzamide; The lithium salt is any one of lithium difluorooxalate borate or lithium difluorosulfate borate; The crown ether compound is any one of 12-crown-4, 18-crown-6 or 15-crown-5; The carbonate compound is any one or both of fluoroethylene carbonate and fluoroethyl methyl carbonate.
2. The wide temperature range electrolyte according to claim 1, characterized in that: The mass ratio of the first component to the second component is 1-2:1-5.
3. The wide temperature range electrolyte according to claim 1, characterized in that: The molar ratio of the lithium salt to the first component in the amide compound is 1:1-1:
5.
4. The wide temperature range electrolyte according to claim 1, characterized in that: The mass ratio of the additive to the lithium salt / amide compound deep eutectic solvent is 0.5:100-5:
100.
5. The wide temperature range electrolyte according to claim 1, characterized in that: The preparation method of the lithium salt / amide compound deep eutectic solvent comprises the following steps: in a dry, low-oxygen environment, the lithium salt and the amide compound are uniformly mixed, and stirred at 60° C.-70° C. until the solution is clear and transparent, to obtain the lithium salt / amide compound deep eutectic solvent.
6. The wide temperature range electrolyte according to claim 5, characterized in that: The water content and oxygen content of the dry, low-oxygen environment are both ≤ 0.1 ppm.
7. A method for preparing a wide temperature range electrolyte according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: uniformly mixing the lithium salt / amide compound deep eutectic solvent and additives to obtain the wide temperature range electrolyte.
8. Use of the wide temperature range electrolyte according to any one of claims 1 to 6 in a lithium ion battery.