A multi-layer coated luminous material, luminous decorative effect ceramic tile and preparation method thereof

By evenly adhering silicate luminescent powder to the surface of aluminate luminescent particles and covering it with high-temperature transparent glaze powder, the problem of poor resistance of ceramic tiles at high temperatures is solved, and efficient luminous characteristics improvement and process simplification are achieved.

CN118324407BActive Publication Date: 2024-10-01MONALISA GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410766200.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01
Estimated Expiration
2044-06-14

Smart Images

  • Figure CN118324407B_ABST
    Figure CN118324407B_ABST
Patent Text Reader

Abstract

The present invention relates to a multi-layer coated luminescent material, a luminescent decorative effect ceramic tile and a preparation method thereof, and belongs to the technical field of ceramic tiles. The multi-layer coated luminescent material comprises a coating in which silicate luminescent powder is uniformly adhered to the surface of aluminate luminescent particles, and a high-temperature transparent glaze powder covering the coating; the silicate luminescent powder is a rare earth doped silicate system luminescent material; the aluminate luminescent particles are rare earth activated alkaline earth aluminate luminescent materials; the mass ratio of the aluminate luminescent particles to the silicate luminescent powder is 60~80:20~40; the initial melting temperature of the high-temperature transparent glaze powder is 1122~1161°C; the mass ratio of the coating to the high-temperature transparent glaze powder is 60~80:20~40. The present invention uses the above-mentioned multi-layer coated luminescent material, and the obtained ceramic tile has a smooth glaze surface and a high-efficiency luminescent decorative effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a multi-layer coated luminescent material, luminescent decorative effect ceramic tile and a preparation method thereof, belonging to the technical field of ceramic tiles. Background Art

[0002] Photoluminescent ceramic tiles can absorb visible light such as sunlight or lamplight and store the light energy. When the light excitation stops, the stored energy is slowly released in the form of light. Due to the advantages of ultra-long afterglow, high brightness, long luminous time, and no radioactivity, photoluminescent ceramic tiles can be used not only for building decoration facilities, warning signs for safe passages in public places, but also for concealed lighting and low-level emergency lighting, bringing great convenience to people's night life and engineering operations.

[0003] At present, the luminescent materials commonly used in building ceramics are mainly rare earth doped aluminate luminescent materials and silicate luminescent materials. Aluminate luminescent materials have long afterglow time, high luminous efficiency, and high initial brightness, but they are unstable when exposed to water, have poor chemical stability, and poor high temperature resistance. They will lose their luminous ability at high temperatures above about 900°C, and are prone to glaze cracking defects. They are mostly used in low-temperature multiple firing processes (such as second firing and third firing). Silicate luminescent materials have good high temperature resistance, the highest firing temperature can reach 1150°C, and the glaze surface is flat and smooth, but the initial luminous brightness is low and the afterglow time is insufficient. They are mainly used in high-temperature single firing processes.

[0004] Chinese patent CN107651949B discloses a luminescent ceramic glazed tile and its preparation method, which comprises a body layer, a base glaze layer, a flower glaze layer, a luminescent layer and a polishing glaze layer from bottom to top. The luminescent layer is made of rare earth-doped Sr4A14O with a particle size of 80 to 120 meshes. 25 , SrAl2O4, Sr2MgSi2O7, CaA12O4, CaTiO3 and at least one luminescent powder. After the surface of the coarse-grained luminescent powder is corroded, the inside of the luminescent powder still has the luminescent property, which overcomes the problem that the traditional luminescent powder is easily corroded by the high-temperature flux, destroying the internal structure of the luminescent powder and causing the luminescent powder to fail. On the other hand, the coarse-grained luminescent powder also has the characteristics of anti-slip particles, and the surface of the ceramic glazed tiles is softly polished to give the luminescent ceramic glazed tiles an anti-slip function. In other words, this scheme uses luminescent powder with coarser particles. Although it overcomes the problem that the traditional luminescent powder is easily corroded by the high-temperature flux and causes the luminescent powder to fail, the glaze surface is uneven after polishing, so it has a certain anti-slip function. In addition, this scheme uses a single luminescent material, and after the glaze surface is corroded, the afterglow time and brightness will be reduced.

[0005] Chinese patent CN106277791B discloses a method for preparing a high-temperature resistant silicate luminescent ceramic glaze, which is to disperse the powder of rare earth activated alkaline earth metal silicate luminescent material into a coating material solution to form a suspension, or gradually add the coating material to the luminescent powder suspension, and after the coating material forms a coating layer on the surface of the luminescent powder, centrifuge the remaining solution, wash it alternately with deionized water and ethanol, dry it, complete the first coating, and then pre-sinter it in the range of 200℃ to 700℃ according to the characteristics of the coating layer, and then cool it for the second coating. The coating material is one or more of ethyl orthosilicate, sodium silicate, aluminum nitrate nonahydrate, zirconium sol and silica sol, and the coating layer is composed of at least one layer of silicon dioxide, aluminum oxide, and zirconium silicate. This scheme coats the silicate luminescent powder twice, which improves the high temperature resistance of the silicate luminescent ceramic glaze. However, although this solution improves the luminous intensity at high temperatures, since only one luminescent material, silicate luminescent powder, is used, the afterglow time of the phosphor cannot be further improved, and the packaging process is complicated. Summary of the invention

[0006] In view of the above problems, the present invention provides a multi-layer coated luminescent material with stable chemical properties, high initial brightness after short-time excitation, long afterglow time, good high temperature resistance and simple preparation process. In addition, the present invention also provides a luminescent decorative effect ceramic tile and a preparation method thereof, which uses the above multi-layer coated luminescent material and has a smooth glaze surface and efficient luminescent decorative effect.

[0007] In the first aspect, the present invention provides a multi-layer coated luminescent material. The multi-layer coated luminescent material comprises a coating in which silicate luminescent powder is uniformly adhered to the surface of aluminate luminescent particles, and a high-temperature transparent glaze powder covering the coating; the silicate luminescent powder is a rare earth doped silicate luminescent material; the aluminate luminescent particles are rare earth activated alkaline earth aluminate luminescent materials; the mass ratio of the aluminate luminescent particles to the silicate luminescent powder is 60~80:20~40; the initial melting temperature of the high-temperature transparent glaze powder is 1122~1161℃; the mass ratio of the coating to the high-temperature transparent glaze powder is 60~80:20~40.

[0008] Preferably, the silicate luminescent powder comprises Sr2MgSi2O7:Eu 2+ ,Dy 3+ 、Ca3MgSi2O8:Eu 2+ ,Dy 3+ 、Ba3MgSi2O8:Eu 2+ ,Dy 3+ At least one of .

[0009] Preferably, the aluminate luminescent particles include SrAI2O4:Eu 2+、SrAI2O4:Eu 2+ ,Dy 3+ 、Sr4AI 14 O 25 :Eu 2 + ,Dy 3+ 、BaAI2O4:Eu 2+ ,Dy 3+ At least one of .

[0010] Preferably, the chemical composition of the high-temperature transparent glaze powder includes, by mass percentage, SiO2: 56~62%, Al2O3: 17~22%, CaO: 7.2~14%, ZnO: 0.8~3.1%, K2O: 0.8~2.1%, Na2O: 2.3~4.0%, MgO: 1.7~2.8%, and BaO: 1.7~6.8%.

[0011] Preferably, the mesh number of the silicate luminescent powder is 290-350 meshes; the mesh number of the aluminate luminescent particles is 200-230 meshes.

[0012] In a second aspect, the present invention provides a method for preparing a multilayer coated luminescent material. The preparation method comprises:

[0013] The silicate luminescent powder and the first binder aqueous solution are mixed evenly and sieved to obtain a silicate luminescent powder with adhesiveness;

[0014] The aluminate luminescent particles and the silicate luminescent powder with adhesiveness are mixed evenly, sieved and dried to obtain a coating body in which the silicate luminescent powder is evenly adhered to the surface of the aluminate luminescent particles;

[0015] The high temperature transparent glaze powder and the second binder aqueous solution are mixed evenly and then sieved to obtain the high temperature transparent glaze powder with adhesiveness;

[0016] The coating body in which the silicate luminescent powder is uniformly adhered to the surface of the aluminate luminescent particles and the high-temperature transparent glaze powder with adhesiveness are evenly mixed, sieved and dried to obtain a multi-layer coated luminescent material.

[0017] Preferably, the first binder and the second binder are independently selected from one or more of acrylic resin, sodium carboxymethyl cellulose, and perchloroethylene; the mass fraction of the first binder aqueous solution is 1.0-3.0%; the mass fraction of the second binder aqueous solution is 1.0-3.0%.

[0018] Preferably, the mass ratio of the first binder aqueous solution to the silicate luminescent powder is 0.2-0.6:100; the mass ratio of the second binder aqueous solution to the high-temperature transparent glaze powder is 0.2-0.6:100.

[0019] In a third aspect, the present invention provides a method for preparing a luminous decorative ceramic tile. The method comprises: applying the multi-layer coated luminous material on a tile blank having an inkjet pattern layer; applying glaze on the surface of the tile blank after applying the multi-layer coated luminous material; the initial melting temperature of the glaze is 1000-1150°C; and firing and polishing the glazed tile blank.

[0020] Preferably, the specific gravity of the glaze is 1.82-1.85 g / cm 3 , glaze application amount is 360~470g / m 2 .

[0021] In a fourth aspect, the present invention provides a method for preparing a luminescent decorative ceramic tile. The preparation method comprises: adding the multi-layer coated luminescent material to the polishing glaze and mixing them evenly to obtain the luminescent ceramic glaze; the initial melting temperature of the polishing glaze is 1000-1150°C; applying the luminescent ceramic glaze to a brick blank having an inkjet pattern layer; and firing and polishing the brick blank after applying the luminescent ceramic glaze.

[0022] Preferably, the specific gravity of the luminescent ceramic glaze is 1.58-1.65 g / cm 3 , glaze application amount is 660~750g / m 2 .

[0023] Preferably, the firing temperature is 1100-1200° C., and the firing period is 42-60 min.

[0024] In a fifth aspect, the present invention provides a luminous decorative ceramic tile, which is obtained according to any of the preparation methods described above.

[0025] Beneficial Effects

[0026] The multi-layer coated luminescent material used in the present invention includes a coating in which silicate luminescent powder is uniformly adhered to the surface of aluminate luminescent particles, and a high-temperature transparent glaze powder covering the coating. The use of silicate luminescent powder to coat aluminate luminescent particles can effectively improve the high temperature resistance of aluminate luminescent particles so that they are not decomposed by heat. The high-temperature transparent glaze powder has a high initial melting point and belongs to a silicate system, and can be well combined with silicate luminescent powder and ceramic glaze. The present invention applies the multi-layer coated luminescent material to the preparation of luminescent decorative effect ceramic tiles, which enhances the luminescent properties of the luminescent material and significantly improves the high-temperature stability of the material. The obtained ceramic tiles have a smooth glaze surface and have the advantages of high initial brightness, long afterglow time and good high temperature resistance after a short period of excitation. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a picture of the aluminate luminescent particles of Example 1 taken using a 300-fold magnifying glass;

[0028] Figure 2 This is a picture of the multi-layer coated luminescent material of Example 1 taken with a 300-fold magnifying glass;

[0029] Figure 3 This is a picture showing the effect of the luminous ceramic tile of Example 1 under an incandescent lamp;

[0030] Figure 4 This is a self-luminous effect diagram of the luminous ceramic tile of Example 1 under weak light (indoor lights turned off in the evening);

[0031] Figure 5 This is a brick surface effect diagram of the luminous ceramic brick of comparative example 3;

[0032] Figure 6 This is a rendering of the luminescent particles in the glaze of the luminescent ceramic tile of comparative example 3. DETAILED DESCRIPTION

[0033] The present invention is further described by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention. In the absence of special instructions, each percentage content refers to the percentage content by mass.

[0034] Although aluminate-based luminescent materials have high initial brightness and long afterglow time after short-time excitation, they are unstable when exposed to water and have poor high-temperature resistance. They begin to lose their luminescence ability at around 900°C, and are prone to glaze crack defects when used in combination with ceramic glazes. Silicate-based luminescent materials have good chemical stability, strong water resistance, and good high-temperature resistance. They still have a certain luminescence ability after being subjected to a high temperature of 1150°C, have good binding properties with ceramic glazes, and basically will not form glaze crack defects, but have low initial brightness after excitation. To this end, the present invention provides a multi-layer coated luminescent material, which uses silicate luminescent powder and high-temperature transparent glaze powder to coat aluminate luminescent particles. After short-time excitation, it has the advantages of high initial brightness, long afterglow time, and good high-temperature resistance.

[0035] The multi-layer coated luminescent material comprises a coating in which silicate luminescent powder is uniformly adhered to the surface of aluminate luminescent particles and a high-temperature transparent glaze powder covering the coating.

[0036] The initial melting temperature of the high-temperature transparent glaze powder is 1122-1161°C, preferably 1122-1150°C.

[0037] If the high-temperature transparent glaze powder is replaced with medium-temperature transparent glaze powder or low-temperature transparent glaze powder, the medium-temperature transparent glaze powder or low-temperature transparent glaze powder will become molten during the high-temperature firing process. The molten flux will corrode the luminescent material, causing the luminescent material to decompose and fail to emit light effectively.

[0038] As an example, the chemical composition of the high-temperature transparent glaze powder includes, in mass percentage, SiO2: 56~62%, Al2O3: 17~22%, CaO: 7.2~14%, ZnO: 0.8~3.1%, K2O: 0.8~2.1%, Na2O: 2.3~4.0%, MgO: 1.7~2.8%, and BaO: 1.7~6.8%.

[0039] The silicate luminescent powder is a rare earth doped silicate luminescent material. Preferably, the silicate luminescent powder includes Sr2MgSi2O7:Eu 2+ ,Dy 3+ 、Ca3MgSi2O8:Eu 2+ ,Dy 3+ 、Ba3MgSi2O8:Eu 2+ ,Dy 3+ At least one of .

[0040] The mesh number of the silicate luminescent powder is 290-350 mesh, for example 325 mesh.

[0041] The aluminate luminescent particles are rare earth activated alkaline earth aluminate luminescent materials. Preferably, the aluminate luminescent particles include SrAI2O4:Eu 2+ 、SrAI2O4:Eu 2+ ,Dy 3+ 、Sr4AI 14 O 25 :Eu 2+ ,Dy 3+ 、BaAI2O4:Eu 2+ ,Dy 3+ The aluminate luminescent particles have high brightness and long afterglow time.

[0042] The mesh number of the aluminate luminescent particles is 200-230 meshes. In the present invention, the particle size of the silicate luminescent powder is set to be finer than that of the aluminate luminescent particles, so that the silicate luminescent powder can be coated on the surface of the aluminate luminescent particles.

[0043] The mass ratio of the aluminate luminescent particles to the silicate luminescent powder is 60~80:20~40. The mass ratio of the aluminate luminescent particles to the silicate luminescent powder is controlled within the above range. If the content of the silicate luminescent powder is low, a complete coating layer may not be formed during the coating process of the aluminate luminescent particles, resulting in partial surface exposure of the aluminate luminescent particles. When subjected to high-temperature sintering, these exposed aluminate luminescent particles will lose their luminescent properties due to lack of protection. If the content of the silicate luminescent powder is too high, during the coating process, too much silicate luminescent powder will agglomerate on the surface of the aluminate luminescent particles in large quantities to form an overly thick coating layer. This may not only lead to uneven coating, but also in subsequent production processes, these excess silicate luminescent powders may also fall off.

[0044] The mass ratio of the coating body to the high temperature transparent glaze powder is 60-80:20-40. The mass ratio of the coating body to the high temperature transparent glaze powder is controlled within the above range to avoid the problem of falling off due to the high temperature transparent glaze powder coating layer being too thick or the loss of protection due to the high temperature transparent glaze powder coating layer being too thin.

[0045] If the aluminate luminescent powder is coated on the surface of the silicate luminescent particles, the expected effect of the present invention will not be produced. This is because the high temperature resistance of the aluminate luminescent material is relatively poor. Even if the surface of the aluminate luminescent material is coated with a layer of high temperature transparent glaze powder, it may still lose its luminescence ability or greatly weaken the luminescence effect under high temperature conditions. This results in the luminescent substance of the multi-layer coated luminescent material being only the silicate luminescent material, thereby weakening the luminescence effect.

[0046] The mesh number of the multi-layer coated luminescent material is 180-220 meshes. The larger the mesh number of the multi-layer coated luminescent material, the better the luminescent effect. When the mesh number of the multi-layer coated luminescent material is less than 180 meshes, a convex effect will be formed on the glaze surface, and the surface of the product will be uneven after polishing. When the mesh number of the multi-layer coated luminescent material is greater than 220 meshes, on the one hand, the luminescent effect is weakened, and on the other hand, it is unevenly dispersed when added to the glaze, affecting the overall effect of the product.

[0047] The prior art CN115093249B self-luminous rock board uses a silicate luminescent material of 100~200 mesh, and the particles are relatively coarse. Since the particles of the luminescent material in the prior art CN115093249B are relatively large, the contact area between its surface and the medium-temperature transparent glaze is limited. Even if the medium-temperature transparent glaze corrodes its surface, the internal structure of the luminescent particles can still maintain its luminescent properties. However, in the present invention, the mesh number of the silicate luminescent powder is 290~350 mesh, the particle size is smaller, and its surface activity is significantly improved. In the high-temperature molten state, the silicate luminescent material is more likely to react with the flux in the medium-temperature transparent glaze; and during the high-temperature firing process, the medium-temperature transparent glaze will reach a completely molten state, the glaze fluidity will be enhanced, and it can be more fully in contact with the silicate luminescent material, thereby affecting the luminescent performance.

[0048] The following is an exemplary description of the method for preparing the multi-layer coated luminescent material of the present invention.

[0049] The silicate luminescent powder and the first binder aqueous solution are mixed evenly and sieved to obtain a silicate luminescent powder with adhesiveness. The mixing method of the silicate luminescent powder and the first binder aqueous solution is not limited. For example, the first binder aqueous solution is evenly sprayed on the silicate luminescent powder, stirred and mixed evenly, and then sieved to obtain a silicate luminescent powder with adhesiveness. It can be sieved through a 250-300 mesh sieve. For example, sieved through a 250 mesh sieve.

[0050] The first binder may be a commonly used binder in the ceramic field. The first binder includes but is not limited to acrylic resin, sodium carboxymethyl cellulose, vinyl chloride, etc. The mass fraction of the first binder aqueous solution may be 1.0-3.0%.

[0051] The mass ratio of the first binder aqueous solution to the silicate luminescent powder is 0.2-0.6: 100. If the amount of the first binder is too little, the powder will have insufficient bonding strength and will not be able to completely coat the luminescent material; if the amount of the first binder is too much, the powder will agglomerate, making the coating process difficult and the particles will be coarse.

[0052] After the aluminate luminescent particles and the silicate luminescent powder with adhesiveness are mixed evenly, the mixture is sieved and dried to obtain a coating. The drying temperature can be 110-140°C. The drying time can be 15-30 minutes. The mixture can be sieved through a 180-230 mesh sieve. For example, the mixture can be sieved through a 180 mesh sieve and a 220 mesh sieve in sequence.

[0053] In some embodiments, aluminate luminescent particles are added to adhesive silicate luminescent powder, mixed thoroughly and evenly so that the silicate luminescent powder is evenly adhered to the surface of the aluminate luminescent particles, and then passed through a 180-mesh sieve and a 220-mesh sieve in sequence, the particles on the 220-mesh sieve are taken, and the coating is obtained after drying.

[0054] The high temperature transparent glaze powder and the second binder aqueous solution are mixed evenly and then sieved to obtain a high temperature transparent glaze powder with adhesiveness. The mixture may be sieved through a 250-300 mesh sieve. For example, sieved through a 250 mesh sieve. The mixing method of the high temperature transparent glaze powder and the second binder aqueous solution is not limited. For example, the second binder aqueous solution is evenly sprayed on the high temperature transparent glaze powder, stirred and mixed evenly, and then sieved through a 250 mesh sieve to obtain a high temperature transparent glaze powder with adhesiveness.

[0055] The second binder may be a binder commonly used in the ceramic field. The second binder includes but is not limited to acrylic resin, sodium carboxymethyl cellulose, perchloroethylene, etc. The mass fraction of the second binder aqueous solution may be 1.0-3.0%.

[0056] The mass ratio of the second binder aqueous solution to the high temperature transparent glaze powder is 0.2-0.6: 100. If the amount of the second binder is too little, the powder will have insufficient bonding strength and will not be able to completely coat the high temperature transparent glaze powder; if the amount of the second binder is too much, the powder will agglomerate, making the coating process difficult and the particles will be coarse.

[0057] The coating body and the high temperature transparent glaze powder with adhesiveness are mixed evenly, sieved and dried to obtain a multi-layer coated luminescent material. The drying temperature can be 110-140°C and the drying time can be 15-30 minutes.

[0058] For example, the coating is added to the high-temperature transparent glaze powder with adhesiveness, mixed thoroughly and evenly, so that the high-temperature transparent glaze powder is evenly adhered to the surface of the coating, and passed through 180 mesh and 220 mesh sieves in turn, the particles on the 220 mesh sieve are taken, and dried at 110~140℃ for 15~30 minutes to obtain a multi-layer coated luminescent material.

[0059] In summary, in order to ensure that the silicate luminescent powder can be coated on the aluminate luminescent particles, the present invention has, on the one hand, a smaller particle size of the silicate luminescent material than the aluminate luminescent particles, and the smaller the particle size, the more conducive to coating, but the luminescent performance is poor when the particle size is too small. The use of silicate-based luminescent materials to coat aluminate-based luminescent materials can effectively improve the high temperature resistance of aluminate-based luminescent materials, so that they are not decomposed by heat. The high-temperature transparent glaze powder has a high initial melting temperature and belongs to the silicate system, and can be well combined with silicate-based luminescent materials and ceramic glazes. The use of high-temperature transparent glaze powder to coat the luminescent material can, on the one hand, isolate the luminescent material from the outside world, thereby protecting the luminescent material from being corroded by the molten glaze, and on the other hand, can make the luminescent material well combined with conventional ceramic glazes, and the high-temperature transparent glaze has excellent translucency, which can not only fully transmit light, but also ensure that the luminescent material maintains its original high brightness. The multi-layer coated luminescent material prepared by the present invention has a fine mesh number, which enhances the luminescent characteristics of the luminescent material, significantly improves the high-temperature stability of the material, and the glaze surface of the ceramic tile prepared is smooth.

[0060] The following is an exemplary description of the method for preparing the luminous decorative ceramic tile of the present invention.

[0061] The multi-layer coated luminescent material is applied to the brick blank with the inkjet pattern layer. The multi-layer coated luminescent material can be applied by a digital glue dry granulator. For example, the multi-layer coated luminescent material is positioned and applied by a digital glue dry granulator, and then the multi-layer coated luminescent material is fixed by spraying a glue fixing agent, and after being fixed, the excess multi-layer coated luminescent material is removed by a blower.

[0062] Glaze is applied on the surface of the brick after multiple layers of luminous material are coated.

[0063] The initial melting temperature of the polishing glaze is 1000-1150° C., preferably 1050-1100° C. The initial melting temperature of the polishing glaze is lower than the initial melting temperature of the high-temperature transparent glaze and the highest heat-resistant temperature of the silicate luminescent powder. The polishing glaze first melts during the high-temperature firing process and covers the surface of the multi-layer coated luminescent material, thereby protecting the luminescent material from oxidation.

[0064] The polishing glaze commonly used in the art can be used. For example, but not limited to, the chemical composition of the polishing glaze includes: in mass percentage, SiO2: 50-56%, Al2O3: 13-17%, CaO: 7.1-14%, ZnO: 2.7-4.0%, K2O: 2.8-3.3%, Na2O: 1.7-4.6%, MgO: 3.1-7.6%, BaO: 4.0-8.9%.

[0065] The glaze is applied by pouring. The specific gravity of the glaze is 1.82-1.85 g / cm 3 , glaze application amount is 360~470 g / m 2 . During the glazing process, the glaze has a low specific gravity and the glaze slurry is too fluid, which leads to unstable glazing and defects such as ripples and flow marks on the brick surface; the glaze has a high specific gravity and the glaze slurry has poor fluidity, so the glaze is not easy to flow on the bell jar, which may lead to uneven glaze layer and even cracking of the glaze surface. Moreover, during the glazing process, the amount of glaze applied is small, and the glaze layer on the brick surface is thin, which may lead to poor polishing effect in the subsequent polishing process; the amount of glaze applied is large, the water content of the brick is high, and the brick is easy to crack during the operation of the production line. During the firing process, the water and gas inside the glaze layer are difficult to be completely discharged, which may cause the product to "explode".

[0066] It is also possible to add a multi-layer coated luminescent material to the polishing glaze and stir and mix evenly to obtain a luminescent ceramic glaze. The mass percentage of the multi-layer coated luminescent material in the polishing glaze can be 30-45%. The initial melting temperature of the polishing glaze is 1000-1150°C, preferably 1050-1100°C. The initial melting temperature of the polishing glaze is lower than the initial melting temperature of the high-temperature transparent glaze and the highest heat-resistant temperature of the silicate luminescent powder. The polishing glaze first melts and covers the surface of the multi-layer coated luminescent material during the high-temperature firing process, thereby protecting the luminescent material from oxidation. The polishing glaze commonly used in the art can be used. For example, but not limited to this, the chemical composition of the polishing glaze includes: in mass percentage, SiO2: 50-56%, Al2O3: 13-17%, CaO: 7.1-14%, ZnO: 2.7-4.0%, K2O: 2.8-3.3%, Na2O: 1.7-4.6%, MgO: 3.1-7.6%, BaO: 4.0-8.9%. Then the luminescent ceramic glaze is applied to the brick blank with the inkjet pattern layer. The luminescent ceramic glaze is applied by spraying. The specific gravity of the luminescent ceramic glaze is 1.58-1.65 g / cm 3 , glaze application amount is 660~750g / m 2 .

[0067] Enter the kiln for firing. The firing temperature is 1100~1200℃ and the firing cycle is 42~60min.

[0068] Polishing after leaving the kiln. Use elastic grinding blocks commonly used in the ceramic industry for bright polishing or soft polishing.

[0069] Edging.

[0070] The present invention provides a luminescent decorative ceramic tile based on aluminate and silicate composite modified materials and a preparation method thereof. After light excitation, the aluminate luminescent material begins to emit light by itself in the absence of light or weak light conditions, and its high initial brightness can further excite the silicate luminescent powder, and the luminescent time is complemented by the composite, thereby significantly improving the afterglow time of the multi-layer coated luminescent material.

[0071] The present invention is further illustrated by the following embodiments. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values ​​​​exemplified below.

[0072] Example 1

[0073] The preparation method of the luminous decorative effect ceramic tile comprises the following steps:

[0074] (1) Sr2MgSiO2O7:Eu 2+ ,Dy 3+ The luminescent powder and 1.0% sodium carboxymethyl cellulose aqueous solution were mixed evenly in a mass ratio of 100:0.2 and then passed through a 250-mesh sieve to obtain a silicate luminescent powder with adhesiveness. 2+ ,Dy 3+ The mesh number of the luminescent powder is 320 mesh.

[0075] (2) SrAI2O4:Eu 2+ The luminescent particles and the silicate luminescent powder with adhesiveness are fully mixed in a mass ratio of 60:40, so that the silicate luminescent powder is evenly adhered to the surface of the aluminate luminescent particles, and then sieved through 180 mesh and 200 mesh sieves in turn. The particles on the 200 mesh sieve are taken and dried at 110°C for 30 minutes to obtain the coating. SrAI2O4:Eu 2+ The mesh number of the luminous particles is 220 mesh.

[0076] (3) High temperature transparent glaze powder and 3.0% sodium carboxymethyl cellulose aqueous solution are mixed evenly in a mass ratio of 100:0.3 and then passed through a 250 mesh sieve to obtain a high temperature transparent glaze powder with adhesiveness. The chemical composition of the high temperature transparent glaze powder includes, by mass percentage, SiO2: 61.2%, Al2O3: 17.6%, CaO: 9.1%, ZnO: 2.9%, K2O: 1.7%, Na2O: 2.3%, MgO: 2.3%, and BaO: 2.9%.

[0077] (4) The coating and the high-temperature transparent glaze powder with adhesiveness are fully mixed and uniformly mixed. The mass ratio of the coating and the high-temperature transparent glaze powder is 70:30. The high-temperature transparent glaze powder is uniformly adhered to the surface of the coating. Then, the coating is passed through a 180-mesh sieve and a 200-mesh sieve in turn, and the particles on the 200-mesh sieve are taken and dried at 110°C for 30 minutes to obtain a multi-layer coated luminescent material.

[0078] (5) The multi-layer coated luminescent material is applied onto the brick blank with the inkjet pattern layer using a digital glue dry granulator.

[0079] (6) Apply glaze to the surface of the brick after applying multiple layers of coated luminescent materials. The chemical composition of the glaze includes: in mass percentage, SiO2: 55.7%, Al2O3: 16.8%, CaO: 12.3%, ZnO: 2.8%, K2O: 2.9%, Na2O: 1.9%, MgO: 3.3%, BaO: 4.3%. The glaze is applied by bell jar glazing. The specific gravity of the glaze is 1.85g / cm 3 , glaze application amount is 470g / m 2 .

[0080] (7) Enter the kiln for firing. The firing temperature is 1200℃ and the firing cycle is 42 minutes.

[0081] (8) After leaving the kiln, the edges are polished and ground to obtain the finished ceramic tile with luminous decorative effect.

[0082] Figure 1 This is the SEM image of the aluminate luminescent particles of Example 1. Figure 2 This is a SEM image of the multi-layer coated luminescent material of Example 1. It can be seen that the silicate luminescent powder forms a complete and uniform coating layer on the surface of the aluminate luminescent particles.

[0083] Figure 3 This is a picture showing the effect of the luminescent ceramic tile of Example 1 under an incandescent lamp. Figure 4 This is a self-luminous effect diagram of the luminous ceramic tile of Example 1 under weak light (indoor lights turned off in the evening). It can be seen that the luminous ceramic tile can emit light by itself under weak light conditions.

[0084] The luminous ceramic tile obtained in Example 1 was placed under 455 lx illumination (with lights on at night) for 20 minutes and then placed in a dark place. The afterglow time was 5 hours and the initial brightness was 0.38 cd / m 2 It can be seen that the present invention uses multi-layer coated luminescent materials, and uses silicate luminescent powder and high-temperature transparent glaze powder to coat aluminate luminescent particles, which has the advantages of high initial brightness, long afterglow time, and good high temperature resistance after short-time excitation.

[0085] Example 2

[0086] The preparation method of the luminous decorative effect ceramic tile comprises the following steps:

[0087] (1) Ca3MgSi2O8:Eu 2+ ,Dy 3+ The luminescent powder and 3.0% perchlorethylene aqueous solution were mixed evenly in a mass ratio of 100:0.6 and then passed through a 250-mesh sieve to obtain a silicate luminescent powder with adhesiveness. 2+ ,Dy 3+ The mesh number of the luminescent powder is 320 mesh.

[0088] (2) SrAI2O4:Eu 2+ The luminescent particles and the silicate luminescent powder with adhesiveness are fully mixed in a mass ratio of 80:20, so that the silicate luminescent powder is evenly adhered to the surface of the aluminate luminescent particles, and then sieved through 180 mesh and 200 mesh sieves in turn. The particles on the 200 mesh sieve are taken and dried at 140°C for 15 minutes to obtain the coating. SrAI2O4:Eu 2+ The mesh number of the luminous particles is 220 mesh.

[0089] (3) High temperature transparent glaze powder and 2.5% perchlorethylene aqueous solution are mixed uniformly in a mass ratio of 100:0.6 and then passed through a 250 mesh sieve to obtain a high temperature transparent glaze powder with adhesiveness. The chemical composition of the high temperature transparent glaze powder includes, by mass percentage, SiO2: 59.4%, Al2O3: 20.1%, CaO: 8.9%, ZnO: 1.1%, K2O: 1.4%, Na2O: 3.6%, MgO: 1.8%, and BaO: 3.7%.

[0090] (4) The coating and the high-temperature transparent glaze powder with adhesiveness are fully mixed and uniformly mixed. The mass ratio of the coating and the high-temperature transparent glaze powder is 80:20. The high-temperature transparent glaze powder is uniformly adhered to the surface of the coating. Then, the coating is sieved with 180 mesh and 200 mesh sieves in turn, and the particles on the 200 mesh sieve are taken and dried at 140°C for 15 minutes to obtain a multi-layer coated luminescent material.

[0091] (5) Add the multi-layer coated luminescent material to the polishing glaze and stir and mix evenly to obtain a luminescent ceramic glaze. The mass percentage of the multi-layer coated luminescent material in the polishing glaze is 45%. The chemical composition of the polishing glaze includes: in mass percentage, SiO2: 51.4%, Al2O3: 14.1%, CaO: 7.7%, ZnO: 3.8%, K2O: 3.1%, Na2O: 4.5%, MgO: 7.1%, BaO: 8.3%.

[0092] (6) Applying the luminescent ceramic glaze on the surface of the brick with the inkjet pattern layer. The luminescent ceramic glaze is applied by spraying. The specific gravity of the luminescent ceramic glaze is 1.60 g / cm 3 , glaze application amount is 670g / m 2 .

[0093] (7) Enter the kiln for firing. The firing temperature is 1150℃ and the firing cycle is 60 minutes.

[0094] (8) After leaving the kiln, the edges are polished and ground to obtain ceramic tiles with luminous decorative effects.

[0095] The tile obtained in Example 2 was placed in a dark place under 1643 lx illumination (bright room) for 15 minutes and then placed in a dark place for 7 hours. The initial brightness was 0.55 cd / m 2 It can be seen that the present invention uses multi-layer coated luminescent materials, and uses silicate luminescent powder and high-temperature transparent glaze powder to coat aluminate luminescent particles, which has the advantages of high initial brightness, long afterglow time, and good high temperature resistance after short-time excitation.

[0096] Comparative Example 1

[0097] The preparation method of the luminous decorative effect ceramic tile comprises the following steps:

[0098] (1) High temperature transparent glaze powder and 1.0% sodium carboxymethyl cellulose aqueous solution are mixed uniformly in a mass ratio of 100:0.3 and then passed through a 250 mesh sieve to obtain a high temperature transparent glaze powder with adhesiveness. The chemical composition of the high temperature transparent glaze powder includes, by mass percentage, SiO2: 61.2%, Al2O3: 17.6%, CaO: 9.1%, ZnO: 2.9%, K2O: 1.7%, Na2O: 2.3%, MgO: 2.3%, and BaO: 2.9%.

[0099] (2) The silicate system Sr2MgSiO2O7:Eu 2+ ,Dy 3+ The luminescent material and the high temperature transparent glaze powder with adhesiveness are fully mixed. Silicate system Sr2MgSiO2O7:Eu 2+ ,Dy 3+ The mesh number of the luminescent material is 180 mesh. Silicate system Sr2MgSiO2O7:Eu 2+ ,Dy 3+ The mass ratio of the luminescent material to the high temperature transparent glaze powder is 70:30. The high temperature transparent glaze powder is uniformly adhered to the silicate system Sr2MgSiO2O7:Eu 2+ ,Dy 3+ The surface of the luminescent material is then sieved through 180 mesh and 200 mesh sieves in turn, the particles on the 200 mesh sieve are taken out, and dried at 110°C for 30 minutes to obtain the coated luminescent material.

[0100] (3) The coated luminescent material is applied onto the brick with the inkjet pattern layer using a digital glue dry granulator.

[0101] (4) Apply glaze to the surface of the brick after the coated luminescent material is applied. The chemical composition of the glaze includes: in mass percentage, SiO2: 55.7%, Al2O3: 16.8%, CaO: 12.3%, ZnO: 2.8%, K2O: 2.9%, Na2O: 1.9%, MgO: 3.3%, BaO: 4.3%. The glaze is applied by bell jar glazing. The specific gravity of the glaze is 1.85g / cm 3 , glaze application amount is 470g / m 2 .

[0102] (5) Enter the kiln for firing. The firing temperature is 1200℃ and the firing cycle is 42 minutes.

[0103] (6) After leaving the kiln, the edges are polished and ground to obtain the finished ceramic tile with luminous decorative effect.

[0104] The tile obtained in comparative example 1 was placed in a dark place under 1754 lx illumination (bright room) for 20 minutes and then placed in a dark place for 3 hours. The initial brightness was 0.13 cd / m 2 It can be seen that the initial brightness value of the ceramic tile of Comparative Example 1 is significantly reduced, and the afterglow time is significantly shortened.

[0105] Comparative Example 2

[0106] The preparation method of the luminous decorative effect ceramic tile comprises the following steps:

[0107] (1) High temperature transparent glaze powder and 2.0% sodium carboxymethyl cellulose aqueous solution are mixed uniformly in a mass ratio of 100:0.3 and then passed through a 250 mesh sieve to obtain a high temperature transparent glaze powder with adhesiveness. The chemical composition of the high temperature transparent glaze powder includes, by mass percentage, SiO2: 61.2%, Al2O3: 17.6%, CaO: 9.1%, ZnO: 2.9%, K2O: 1.7%, Na2O: 2.3%, MgO: 2.3%, and BaO: 2.9%.

[0108] (2) Aluminate system Sr4AI 14 O 25 :Eu 2+ ,Dy 3+ The luminescent material and the high temperature transparent glaze powder with adhesiveness are fully mixed. 14 O 25 :Eu 2+ ,Dy 3+ The mesh number of the luminescent material is 180 mesh. Aluminate system Sr4AI 14 O 25 :Eu 2 + ,Dy 3+ The mass ratio of the luminescent material to the high temperature transparent glaze powder is 70:30. The high temperature transparent glaze powder is uniformly adhered to the aluminate system Sr4AI 14 O 25 :Eu 2+ ,Dy 3+ The surface of the luminescent material is then sieved through 180 mesh and 200 mesh sieves in turn, the particles on the 200 mesh sieve are taken out, and dried at 110°C for 30 minutes to obtain the coated luminescent material.

[0109] (3) The coated luminescent material is applied onto the brick with the inkjet pattern layer using a digital glue dry granulator.

[0110] (4) Apply glaze to the surface of the brick after the coated luminescent material is applied. The chemical composition of the glaze includes: in mass percentage, SiO2: 55.7%, Al2O3: 16.8%, CaO: 12.3%, ZnO: 2.8%, K2O: 2.9%, Na2O: 1.9%, MgO: 3.3%, BaO: 4.3%. The glaze is applied by bell jar glazing. The specific gravity of the glaze is 1.85g / cm 3 , glaze application amount is 470g / m 2 .

[0111] (5) Enter the kiln for firing. The firing temperature is 1200℃ and the firing cycle is 42 minutes.

[0112] (6) After leaving the kiln, the edges are polished and ground to obtain the finished ceramic tile with luminous decorative effect.

[0113] In this comparative example 2, due to Sr4AI 14 O 25 :Eu 2+ ,Dy 3+ The luminous particles have poor high temperature resistance. At high temperatures, Sr4AI 14 O 25 :Eu 2+ ,Dy 3+ Eu 2+ Oxidized to Eu 3+ , which causes the product to lose its luminous effect.

[0114] Comparative Example 3

[0115] The preparation method of the luminous decorative effect ceramic tile comprises the following steps:

[0116] (1) The silicate system Sr2MgSiO2O7:Eu with a mesh size of 100 2+ ,Dy 3+ The luminescent material is applied on the brick with the inkjet pattern layer by using a digital glue dry granulator.

[0117] (2) Apply glaze to the surface of the brick after applying the luminescent material. The chemical composition of the glaze includes: in mass percentage, SiO2: 55.7%, Al2O3: 16.8%, CaO: 12.3%, ZnO: 2.8%, K2O: 2.9%, Na2O: 1.9%, MgO: 3.3%, BaO: 4.3%. The glaze is applied by bell jar glazing. The specific gravity of the glaze is 1.85g / cm 3 , glaze application amount is 470g / m 2 .

[0118] (3) Enter the kiln for firing. The firing temperature is 1200℃ and the firing cycle is 42 minutes.

[0119] (4) After leaving the kiln, the edges are polished and ground to obtain the finished ceramic tile with luminous decorative effect.

[0120] Figure 5 This is a brick surface effect diagram of the luminous ceramic brick of comparative example 3. It can be seen that the glaze surface is obviously uneven after firing, and the glaze surface still presents an uneven effect even after polishing.

[0121] Figure 6 This is a rendering of the luminescent particles in the glaze of the luminescent ceramic tile of comparative example 3. It can be seen that an obvious interface appears between the silicate luminescent particles and the glaze, and the luminescent particles block part of the pattern color.

[0122] Comparative Example 4

[0123] The preparation method of the luminous decorative effect ceramic tile comprises the following steps:

[0124] (1) SrAI2O4:Eu 2+ Aluminate luminescent particles, Ca3MgSi2O8:Eu 2+ ,Dy 3+ The silicate luminescent powder and the high temperature transparent glaze powder are uniformly mixed in a mass ratio of 70:30:30 to obtain a mixed material. The chemical composition of the high temperature transparent glaze powder includes: in mass percentage, SiO2: 59.4%, Al2O3: 20.1%, CaO: 8.9%, ZnO: 1.1%, K2O: 1.4%, Na2O: 3.6%, MgO: 1.8%, BaO: 3.7%. The mesh number of the aluminate luminescent particles is 200 mesh. The mesh number of the silicate luminescent powder is 290 mesh.

[0125] (2) Add the mixed material to the polishing glaze and stir to mix evenly to obtain a luminescent ceramic glaze. The mass percentage of the mixed material to the polishing glaze is 45%. The chemical composition of the polishing glaze includes: in mass percentage, SiO2: 51.4%, Al2O3: 14.1%, CaO: 7.7%, ZnO: 3.8%, K2O: 3.1%, Na2O: 4.5%, MgO: 7.1%, BaO: 8.3%.

[0126] (3) Applying the luminescent ceramic glaze on the surface of the brick with the inkjet pattern layer. The luminescent ceramic glaze is applied by spraying. The specific gravity of the luminescent ceramic glaze is 1.60 g / cm 3 , glaze application amount is 670g / m 2 .

[0127] (4) Firing in kiln. The firing temperature is 1150℃ and the firing cycle is 60 minutes.

[0128] (5) After leaving the kiln, the edges are polished and ground to obtain ceramic tiles with luminous decorative effects.

[0129] The tiles obtained in Comparative Example 4 have no luminescent effect. This is because the three materials, aluminate luminescent particles, silicate luminescent powder and high-temperature transparent glaze powder, are simply physically mixed and no specific coating structure is formed on the surface, and the aluminate luminescent particles lose their luminescent properties at high temperatures.

Claims

1. A method for preparing a luminous decorative ceramic tile, characterized in that: The preparation method comprises: applying a multi-layer coated luminescent material on a brick blank having an inkjet pattern layer; applying a glaze on the surface of the brick blank after applying the multi-layer coated luminescent material; the initial melting temperature of the glaze is 1000-1150°C; the specific gravity of the glaze is 1.82-1.85 g / cm 3 , glaze application amount is 360~470g / m 2 ; firing and polishing the glazed brick; the firing temperature is 1100~1200℃, and the firing period is 42~60min; or the preparation method includes: adding multiple layers of coated luminescent materials to the glaze and mixing them evenly to obtain luminescent ceramic glaze; the initial melting temperature of the glaze is 1000~1150℃; applying the luminescent ceramic glaze on the brick with the inkjet pattern layer; the specific gravity of the luminescent ceramic glaze is 1.58~1.65g / cm 3 , glaze application amount is 660~750g / m 2 ; Firing and polishing the bricks after applying the luminous ceramic glaze; the firing temperature is 1100~1200℃, and the firing cycle is 42~60min; The multi-layer coated luminescent material comprises a coating in which silicate luminescent powder is uniformly adhered to the surface of aluminate luminescent particles, and a high-temperature transparent glaze powder covering the coating; the silicate luminescent powder is a rare earth doped silicate luminescent material; the aluminate luminescent particles are rare earth activated alkaline earth aluminate luminescent materials; the mass ratio of the aluminate luminescent particles to the silicate luminescent powder is 60-80:20-40; the initial melting temperature of the high-temperature transparent glaze powder is 1122-1161°C; the coating and the high-temperature The mass ratio of transparent glaze powder is 60~80:20~40; the chemical composition of the high-temperature transparent glaze powder includes: in mass percentage, SiO2: 56~62%, Al2O3: 17~22%, CaO: 7.2~14%, ZnO: 0.8~3.1%, K2O: 0.8~2.1%, Na2O: 2.3~4.0%, MgO: 1.7~2.8%, BaO: 1.7~6.8%; the mesh number of the multi-layer coated luminescent material is 180~220 meshes.

2. The preparation method according to claim 1, characterized in that: The silicate luminescent powder includes Sr2MgSi2O7:Eu 2 + ,Dy 3+ 、Ca3MgSi2O8:Eu 2+ ,Dy 3+ 、Ba3MgSi2O8:Eu 2+ ,Dy 3+ At least one of .

3. The preparation method according to claim 1, characterized in that: The aluminate luminescent particles include SrAI2O4:Eu 2 + 、SrAI2O4:Eu 2+ ,Dy 3+ 、Sr4AI 14 O 25 :Eu 2+ ,Dy 3+ 、BaAI2O4:Eu 2+ ,Dy 3+ At least one of .

4. The preparation method according to claim 1, characterized in that: The mesh number of the silicate luminescent powder is 290-350 meshes; the mesh number of the aluminate luminescent particles is 200-230 meshes.

5. The preparation method according to claim 1, characterized in that: The preparation method of the multi-layer coated luminescent material comprises: The silicate luminescent powder and the first binder aqueous solution are mixed evenly and sieved to obtain a silicate luminescent powder with adhesiveness; The aluminate luminescent particles and the silicate luminescent powder with adhesiveness are mixed evenly, sieved and dried to obtain a coating body in which the silicate luminescent powder is evenly adhered to the surface of the aluminate luminescent particles; The high temperature transparent glaze powder and the second binder aqueous solution are mixed evenly and then sieved to obtain the high temperature transparent glaze powder with adhesiveness; The coating body in which the silicate luminescent powder is uniformly adhered to the surface of the aluminate luminescent particles and the high-temperature transparent glaze powder with adhesiveness are evenly mixed, sieved and dried to obtain a multi-layer coated luminescent material.

6. The preparation method according to claim 5, characterized in that: The first binder and the second binder are independently selected from one or more of acrylic resin, sodium carboxymethyl cellulose, and vinyl chloride; the mass fraction of the first binder aqueous solution is 1.0-3.0%; the mass fraction of the second binder aqueous solution is 1.0-3.0%.

7. The preparation method according to claim 5, characterized in that: The mass ratio of the first binder aqueous solution to the silicate luminescent powder is 0.2-0.6:100; the mass ratio of the second binder aqueous solution to the high-temperature transparent glaze powder is 0.2-0.6:

100.

8. A luminous decorative ceramic tile, characterized in that: The luminous decorative effect ceramic tile is obtained according to the preparation method described in any one of claims 1 to 7.