An EB curing coating and its application on photovoltaic backplane PET film
By using EB curing coating on the photovoltaic backsheet PET film, combined with polycarbonate and polybutadiene modified polyurethane acrylate, the problems of high water vapor transmission rate and poor hydrolysis resistance of the PET film are solved, and efficient weather resistance is achieved And the transparency is improved, the cost is reduced, the high-priced fluorine film is replaced, and the reliability of the backplane is improved.
Patent Information
- Application Number
- CN202410592469.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-14
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-05-14
AI Technical Summary
Existing photovoltaic backsheet PET films have high water vapor transmittance and poor hydrolysis resistance during long-term outdoor use, which leads to hydrolysis and deterioration of the resin and cannot effectively protect the cells. Moreover, the existing modification schemes or fluorine film production are complex and costly. , the performance is unstable.
Using EB cured coatings, including polycarbon-modified polyurethane acrylate and polybutadiene-modified polyurethane acrylate, prepared through specific reaction steps, combined with cyclotrimethylolpropane methyl acrylate and ultraviolet light absorber, It is coated on the corona-treated PET film and cured by electron beam to form a coating to improve the weather resistance and transparency of the backsheet.
It significantly improves the hydrolysis resistance, yellowing resistance and thermal stability of the photovoltaic backsheet PET film, reduces costs, replaces high-priced fluorine films, and improves the reliability and price advantage of the backsheet.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer coatings, and in particular relates to an EB curing coating and application thereof on a photovoltaic backboard PET film. Background Art
[0002] The main structure of a solar cell module is composed of a panel, glue, cells, glue and backplane stacked together. The backplane is the most important structure in a solar cell module except for the cells. The backplane is a packaging material that is directly in contact with the external environment over a large area, and plays a supporting and protective role for the cells. Generally, the service life of a solar cell module is required to be more than 25 years. Such a long service life requirement imposes strict restrictions on the quality of the backplane, which must have reliable weather resistance, water vapor barrier and insulation. At present, the backplane made of polyethylene terephthalate (PET) as the middle layer has become the mainstream photovoltaic backplane on the market due to its advantages such as high strength, good weather resistance and strong thermal stability. However, it still has the disadvantages of high water vapor permeability, poor hydrolysis resistance and moisture and heat resistance. During long-term outdoor use, water vapor and oxygen in the environment will penetrate into the middle layer through the lower surface protective layer of the middle layer PET film, causing the PET film to hydrolyze and deteriorate, and eventually separate from the filling resin, losing the protection and support for the cells.
[0003] In the prior art, there is a scheme for directly modifying the middle layer PET film: PET resin, PP resin, PET functional masterbatch, compatibilizer and antioxidant are mixed evenly in proportion, added to a twin-screw extruder to extrude a cast sheet, and then the cast sheet is statically biaxially stretched to obtain a new PET film; this scheme enables the middle layer PET film to have good weather resistance and hydrolysis resistance, but the compatibility between PET resin and PP resin is not good. Although it can be improved to a certain extent by adding a compatibilizer, there is still a problem of incompatibility, and the transparency of the modified PET film is reduced, and the hydrolysis resistance is not excellent enough, and there is room for further improvement.
[0004] In the prior art, fluorofilm (PVDF) is used to compound or coat one or both sides of the middle layer PET film to make the back panel have good barrier, weather resistance and insulation properties, especially excellent hydrolysis resistance. However, the production process of fluorofilm is complicated and expensive. The raw materials are monopolized by international companies such as Arkema and Solvay. The domestic fluorofilm with price advantage has many shortcomings such as high crystal content, poor yellowing resistance, large batch difference, poor stability and so on. Summary of the invention
[0005] The object of the present invention is to provide an EB-cured coating and its application on a photovoltaic backplane PET film to solve the problems in the background technology.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] An EB curing coating comprises the following raw materials in parts by weight:
[0008] 10-50 parts of polycarbonate modified polyurethane acrylate, 10-50 parts of polybutadiene modified polyurethane acrylate, 10 parts of cyclotrimethylolpropane formal acrylate, 20 parts of hexanediol diacrylate, 1 part of ultraviolet light absorber, and 0.5 parts of wetting and leveling agent.
[0009] Furthermore, the polycarbon-modified polyurethane acrylate is prepared by the following steps:
[0010] Step A1, adding isophorone diisocyanate and hydroxyethyl acrylate into a three-necked flask while stirring, and after mixing evenly, adding a polymerization inhibitor and an organic bismuth catalyst dropwise while stirring, and controlling the dropping time to be 30 minutes. At the same time, heating the three-necked flask to 70° C., keeping the temperature for reaction for 3.5 hours, and detecting that the NCO content reaches the theoretical value, to obtain a polyurethane prepolymer;
[0011] The reaction process is as follows:
[0012]
[0013] Step A2, adding the preheated polyhexamethylene carbonate diol to the polyurethane prepolymer while stirring, and simultaneously dropping an organic bismuth catalyst, controlling the temperature at 68-72° C. to react for 3 hours, detecting the NCO content to be 0, and obtaining polycarbonate-modified polyurethane acrylate.
[0014] The reaction process is as follows:
[0015]
[0016] Furthermore, in step A1, the molar ratio of isophorone diisocyanate to hydroxyethyl acrylate is 1:1-1.5; the amount of the inhibitor is 0.08-0.1% of the sum of the mass of isophorone diisocyanate and hydroxyethyl acrylate, and the inhibitor is p-hydroxyanisole (MEHQ); the amount of the organic bismuth catalyst is 0.08-0.1% of the sum of the mass of isophorone diisocyanate and hydroxyethyl acrylate.
[0017] Furthermore, in step A2, the molar ratio of polyhexamethylene carbonate diol to polyurethane prepolymer is 1-1.5:2; and the amount of the organic bismuth catalyst is 0.08-0.1% of the sum of the mass of polyhexamethylene carbonate diol and polyurethane prepolymer.
[0018] Furthermore, the polybutadiene-modified polyurethane acrylate is prepared by the following steps:
[0019] Step B1, adding hydroxy-terminated polycis-butadiene and polyether diol into a three-necked flask, vacuum dehydrating for 1 hour, adding isophorone diisocyanate, stirring and heating to 70° C. and keeping the temperature for reaction for 30 minutes, then adding a chelated tin catalyst, heating to 80° C., continuing stirring and keeping the temperature for reaction for 1.5-2 hours, to obtain a polybutadiene-modified polyurethane prepolymer;
[0020] Step B2, adding 1,4-butanediol to the polybutadiene-modified polyurethane prepolymer, maintaining the temperature at 80° C. for 1 hour, then adding hydroxyethyl acrylate and a chelated tin catalyst, and performing a capping reaction for 2 hours to obtain polybutadiene-modified polyurethane acrylate.
[0021] Furthermore, in step B1, the molar ratio of the hydroxy-terminated polycis-butadiene, polyether diol and isophorone diisocyanate is 5-8:2-5:20; the amount of the chelated tin catalyst is 0.08-0.1% of the sum of the mass of the hydroxy-terminated polycis-butadiene, polyether diol and isophorone diisocyanate.
[0022] Furthermore, in step B2, the molar ratio of the polybutadiene-modified polyurethane prepolymer, 1,4-butanediol and hydroxyethyl acrylate is 2:1-2:4; the amount of the chelated tin catalyst is 0.08-0.1% of the sum of the masses of the polybutadiene-modified polyurethane prepolymer, 1,4-butanediol and hydroxyethyl acrylate.
[0023] Furthermore, the ultraviolet light absorber is hydroxyphenyl triazine (HPT); and the wetting and leveling agent is polyether-modified polydimethylsiloxane.
[0024] Furthermore, the preparation method of the EB curing coating is:
[0025] Polycarbonate-modified polyurethane acrylate, polybutadiene-modified polyurethane acrylate, cyclotrimethylolpropane formal acrylate, hexanediol diacrylate, ultraviolet light absorber and wetting and leveling agent are weighed in sequence according to the formula ratio, then added into a disperser, and dispersed at a speed of 500-1000r / min for 5 minutes to obtain an EB-cured coating.
[0026] An application of an EB curing coating on a photovoltaic backplane PET film comprises the following steps:
[0027] The EB curing coating is coated on the corona treated PET film using a 30um wire rod, and then cured by an electron beam curing device to form a coating to obtain a photovoltaic backplane PET film.
[0028] Furthermore, the curing voltage is 180-200 KeV, and the curing dose is 30-40 kGy.
[0029] Beneficial effects:
[0030] The invention firstly uses hydroxyethyl acrylate and isophorone diisocyanate to carry out nucleophilic addition reaction to obtain a polyurethane prepolymer, and then carries out nucleophilic addition reaction with polyhexamethylene carbonate diol to obtain a polycarbonate-modified polyurethane acrylate, so that the polycarbonate-modified polyurethane acrylate has excellent hardness, hydrolysis resistance, thermal stability, weather resistance and chemical resistance.
[0031] The present invention further uses terminal hydroxyl polycis-butadiene and polyether diol to react with isophorone diisocyanate to obtain a polybutadiene-modified polyurethane prepolymer, and then uses 1,4-butanediol to extend the chain and uses hydroxyethyl acrylate to perform end-capping to obtain a polybutadiene-modified polyurethane acrylate, so that the polybutadiene-modified polyurethane acrylate has good transparency, yellowing resistance and low temperature resistance.
[0032] The present invention uses polycarbonate-modified polyurethane acrylate, polybutadiene-modified polyurethane acrylate and cyclotrimethylolpropane formal acrylate in combination, and various performances are synergistically promoted to obtain an EB-cured coating with excellent performance, and the cost is low and has a price advantage; the EB-cured coating is coated on a PET film after corona treatment, and after being cured by an electron beam curing device, a photovoltaic backboard PET film is obtained, which can replace the use of a fluorine film and improve the reliability of the photovoltaic backboard PET film. DETAILED DESCRIPTION
[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] This embodiment provides a polycarbonate-modified polyurethane acrylate prepared by the following steps:
[0036] Step A1, adding 0.2 mol of isophorone diisocyanate and 0.2 mol of hydroxyethyl acrylate into a three-necked flask while stirring, and after mixing evenly, adding 0.08% of the total mass of the above raw materials, p-hydroxyanisole and 0.08% of the organic bismuth catalyst while stirring, controlling the dropping time to 30 minutes, and heating the three-necked flask to 70° C., keeping the temperature for reaction for 3.5 hours, detecting the NCO content to reach the theoretical value, and obtaining a polyurethane prepolymer;
[0037] Step A2, adding the preheated 0.1 mol of hexamethylene carbonate diol to 0.2 mol of polyurethane prepolymer while stirring, and at the same time, adding 0.08% of the total mass of the above raw materials as an organic bismuth catalyst, controlling the temperature at 68°C to react for 3 hours, detecting the NCO content to be 0, and obtaining polycarbonate-modified polyurethane acrylate.
[0038] Example 2
[0039] This embodiment provides a polycarbonate-modified polyurethane acrylate prepared by the following steps:
[0040] Step A1, adding 0.2 mol of isophorone diisocyanate and 0.25 mol of hydroxyethyl acrylate into a three-necked flask while stirring, and after mixing evenly, adding dropwise 0.09% of the total mass of the above raw materials, p-hydroxyanisole and 0.09% of an organic bismuth catalyst while stirring, controlling the dropping time to be 30 min, and heating the three-necked flask to 70° C., keeping the temperature for reaction for 3.5 hours, and detecting that the NCO content reaches the theoretical value, to obtain a polyurethane prepolymer;
[0041] Step A2, adding the preheated 0.12 mol of hexamethylene carbonate diol to 0.2 mol of polyurethane prepolymer while stirring, and at the same time, adding 0.09% of the total mass of the above raw materials as an organic bismuth catalyst, controlling the temperature at 70°C to react for 3 hours, detecting the NCO content to be 0, and obtaining polycarbonate-modified polyurethane acrylate.
[0042] Example 3
[0043] This embodiment provides a polycarbonate-modified polyurethane acrylate prepared by the following steps:
[0044] Step A1, adding 0.2 mol of isophorone diisocyanate and 0.3 mol of hydroxyethyl acrylate into a three-necked flask while stirring, and after mixing evenly, adding dropwise 0.1% of the total mass of the above raw materials, p-hydroxyanisole and 0.1% of an organic bismuth catalyst while stirring, controlling the dropping time to be 30 min, and heating the three-necked flask to 70° C., keeping the temperature for reaction for 3.5 hours, and detecting that the NCO content reaches the theoretical value, to obtain a polyurethane prepolymer;
[0045] Step A2, add 0.15 mol of preheated polyhexamethylene carbonate diol to 0.2 mol of polyurethane prepolymer while stirring, and at the same time, add 0.1% of the total mass of the above raw materials as an organic bismuth catalyst, control the temperature at 72°C to react for 3 hours, detect the NCO content to be 0, and obtain polycarbonate-modified polyurethane acrylate.
[0046] Example 4
[0047] This embodiment provides a polybutadiene-modified polyurethane acrylate prepared by the following steps:
[0048] Step B1, add 0.08 mol of hydroxy-terminated polycis-butadiene and 0.02 mol of polyether diol into a three-necked flask, vacuum dehydrate for 1 hour, add 0.2 mol of isophorone diisocyanate, stir and heat to 70° C. and keep warm for 30 minutes, then add 0.08% of the total mass of the above raw materials, heat to 80° C., continue stirring and keep warm for 1.5 hours to obtain a polybutadiene-modified polyurethane prepolymer;
[0049] Step B2: add 0.05 mol of 1,4-butanediol to 0.1 mol of polybutadiene-modified polyurethane prepolymer, keep the reaction at 80° C. for 1 hour, then add 0.2 mol of hydroxyethyl acrylate and 0.08% of the total mass of the above raw materials as a chelated tin catalyst, and perform a capping reaction at 80° C. for 2 hours to obtain polybutadiene-modified polyurethane acrylate.
[0050] Example 5
[0051] This embodiment provides a polybutadiene-modified polyurethane acrylate prepared by the following steps:
[0052] Step B1, add 0.06 mol of hydroxy-terminated polycis-butadiene and 0.04 mol of polyether diol into a three-necked flask, vacuum dehydrate for 1 hour, add 0.2 mol of isophorone diisocyanate, stir and heat to 70° C. and keep warm for 30 minutes, then add 0.09% of the total mass of the above raw materials, heat to 80° C., continue stirring and keep warm for 2 hours to obtain a polybutadiene-modified polyurethane prepolymer;
[0053] Step B2: add 0.08 mol of 1,4-butanediol to 0.1 mol of polybutadiene-modified polyurethane prepolymer, keep the reaction at 80° C. for 1 hour, then add 0.2 mol of hydroxyethyl acrylate and 0.09% of the total mass of the above raw materials as a chelated tin catalyst, and perform a capping reaction at 80° C. for 2 hours to obtain polybutadiene-modified polyurethane acrylate.
[0054] Example 6
[0055] This embodiment provides a polybutadiene-modified polyurethane acrylate prepared by the following steps:
[0056] Step B1, add 0.05 mol of hydroxy-terminated polycis-butadiene and 0.05 mol of polyether diol into a three-necked flask, vacuum dehydrate for 1 hour, add 0.2 mol of isophorone diisocyanate, stir and heat to 70° C. and keep warm for 30 minutes, then add 0.1% of the total mass of the above raw materials, heat to 80° C., continue stirring and keep warm for 2 hours to obtain a polybutadiene-modified polyurethane prepolymer;
[0057] Step B2: add 0.1 mol of 1,4-butanediol to 0.1 mol of polybutadiene-modified polyurethane prepolymer, keep the reaction at 80° C. for 1 hour, then add 0.2 mol of hydroxyethyl acrylate and 0.1% of the total mass of the above raw materials as a chelated tin catalyst, and perform a capping reaction at 80° C. for 2 hours to obtain polybutadiene-modified polyurethane acrylate.
[0058] Example 7
[0059] This embodiment provides an EB curing coating, which is prepared by the following method:
[0060] 30 parts by weight of the polycarbonate-modified polyurethane acrylate prepared in Example 1, 30 parts by weight of the polybutadiene-modified polyurethane acrylate prepared in Example 4, 10 parts by weight of cyclotrimethylolpropane formal acrylate, 20 parts by weight of hexanediol diacrylate, 1 part by weight of hydroxyphenyl triazine, and 0.5 parts by weight of polyether-modified polydimethylsiloxane were weighed in sequence, added into a disperser at a speed of 500 r / min, and dispersed for 5 minutes to obtain an EB-cured coating;
[0061] This embodiment also provides the application of the EB curing coating on the photovoltaic backplane PET film, including the following steps:
[0062] The EB curing coating is coated on the corona treated PET film with a 30um wire rod, and then cured by electron beam curing equipment at a voltage of 180KeV and a curing dose of 30kGy to form a coating to obtain a photovoltaic backplane PET film.
[0063] Example 8
[0064] This embodiment provides an EB curing coating, which is prepared by the following method:
[0065] 40 parts by weight of the polycarbonate-modified polyurethane acrylate prepared in Example 2, 20 parts by weight of the polybutadiene-modified polyurethane acrylate prepared in Example 5, 10 parts by weight of cyclotrimethylolpropane formal acrylate, 20 parts by weight of hexanediol diacrylate, 1 part by weight of hydroxyphenyl triazine, and 0.5 parts by weight of polyether-modified polydimethylsiloxane were weighed in sequence, added into a disperser at a speed of 800 r / min, and dispersed for 5 minutes to obtain an EB-cured coating;
[0066] This embodiment also provides the application of the EB curing coating on the photovoltaic backplane PET film, including the following steps:
[0067] The EB curing coating is coated on the corona treated PET film with a 30um wire rod, and then cured by electron beam curing equipment at a voltage of 190KeV and a curing dose of 35kGy to form a coating to obtain a photovoltaic backplane PET film.
[0068] Example 9
[0069] This embodiment provides an EB curing coating, which is prepared by the following method:
[0070] 50 parts by weight of the polycarbonate-modified polyurethane acrylate prepared in Example 3, 10 parts by weight of the polybutadiene-modified polyurethane acrylate prepared in Example 6, 10 parts by weight of cyclotrimethylolpropane formal acrylate, 20 parts by weight of hexanediol diacrylate, 1 part by weight of hydroxyphenyl triazine, and 0.5 parts by weight of polyether-modified polydimethylsiloxane were weighed in sequence, added into a disperser at a speed of 1000 r / min, and dispersed for 5 minutes to obtain an EB-cured coating;
[0071] This embodiment also provides the application of the EB curing coating on the photovoltaic backplane PET film, including the following steps:
[0072] The EB curing coating is coated on the corona treated PET film with a 30um wire rod, and then cured by electron beam curing equipment at a voltage of 200KeV and a curing dose of 40kGy to form a coating to obtain a photovoltaic backplane PET film.
[0073] Example 10
[0074] This embodiment provides an EB curing coating, which is prepared by the following method:
[0075] 10 parts by weight of the polycarbonate-modified polyurethane acrylate prepared in Example 2, 50 parts by weight of the polybutadiene-modified polyurethane acrylate prepared in Example 5, 10 parts by weight of cyclotrimethylolpropane formal acrylate, 20 parts by weight of hexanediol diacrylate, 1 part by weight of hydroxyphenyl triazine, and 0.5 parts by weight of polyether-modified polydimethylsiloxane were weighed in sequence, added into a disperser at a speed of 1000 r / min, and dispersed for 5 minutes to obtain an EB-cured coating;
[0076] This embodiment also provides the application of the EB curing coating on the photovoltaic backplane PET film, including the following steps:
[0077] The EB curing coating is coated on the corona treated PET film with a 30um wire rod, and then cured by electron beam curing equipment at a voltage of 200KeV and a curing dose of 40kGy to form a coating to obtain a photovoltaic backplane PET film.
[0078] Embodiment 11
[0079] This embodiment provides an EB curing coating, which is prepared by the following method:
[0080] 20 parts by weight of the polycarbonate-modified polyurethane acrylate prepared in Example 3, 40 parts by weight of the polybutadiene-modified polyurethane acrylate prepared in Example 6, 10 parts by weight of cyclotrimethylolpropane formal acrylate, 20 parts by weight of hexanediol diacrylate, 1 part by weight of hydroxyphenyl triazine, and 0.5 parts by weight of polyether-modified polydimethylsiloxane were weighed in sequence, added into a disperser at a speed of 1000 r / min, and dispersed for 5 minutes to obtain an EB-cured coating;
[0081] This embodiment also provides the application of the EB curing coating on the photovoltaic backplane PET film, including the following steps:
[0082] The EB curing coating is coated on the corona treated PET film with a 30um wire rod, and then cured by electron beam curing equipment at a voltage of 200KeV and a curing dose of 40kGy to form a coating to obtain a photovoltaic backplane PET film.
[0083] Comparative Example 1
[0084] This comparative example is different from Example 7 in that an equal amount of common commercially available polyurethane acrylate is used to replace the polycarbonate-modified polyurethane acrylate prepared in Example 1 and the polybutadiene-modified polyurethane acrylate prepared in Example 4, and the other raw materials and preparation methods are the same.
[0085] Comparative Example 2
[0086] This comparative example is compared with Example 7, except that an equal amount of common commercially available polyurethane acrylate is used to replace the polybutadiene-modified polyurethane acrylate prepared in Example 4, and the other raw materials and preparation methods are the same.
[0087] Comparative Example 3
[0088] The difference between this comparative example and Example 7 is that an equal amount of common commercially available polyurethane acrylate is used to replace the polycarbonate-modified polyurethane acrylate in Example 1, and the other raw materials and preparation methods are the same.
[0089] Comparative Example 4
[0090] This comparative example is compared with Example 7, except that cyclotrimethylolpropane formal acrylate is not added, and the other raw materials and preparation methods are the same.
[0091] The photovoltaic backplane PET films prepared in Examples 7 to 11 and Comparative Examples 1 to 4 were tested for performance, and the results are shown in Table 1:
[0092] Table 1
[0093]
[0094]
[0095] It can be seen from the data in Table 1 that the photovoltaic backplane PET films prepared in Examples 7 to 11 have excellent hydrolysis resistance, yellowing resistance, and weather resistance, the coating has high adhesion to the substrate, and the transparency can still be maintained at the original level; comparing the results of Example 7 with those of Comparative Examples 1-4, it can be seen that the polycarbonate-modified polyurethane acrylate, polybutadiene-modified polyurethane acrylate, and cyclotrimethylolpropane formal acrylate can synergistically promote each other, and compared with using them alone or separately, all aspects of performance can achieve a significant improvement effect.
[0096] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0097] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An EB curing coating, characterized in that: By weight, it includes the following raw materials: 10-50 parts of polycarbonate modified polyurethane acrylate, 10-50 parts of polybutadiene modified polyurethane acrylate, 10 parts of cyclotrimethylolpropane formal acrylate, 20 parts of hexanediol diacrylate, 1 part of ultraviolet light absorber, and 0.5 parts of wetting and leveling agent; The polycarbon-modified polyurethane acrylate is prepared by the following steps: Step A1, adding isophorone diisocyanate and hydroxyethyl acrylate into a three-necked flask while stirring, and after mixing evenly, adding a polymerization inhibitor and an organic bismuth catalyst dropwise while stirring, and controlling the dropping time to be 30 minutes. At the same time, the three-necked flask is heated to 70° C. and reacted for 3.5 hours to obtain a polyurethane prepolymer; Step A2, adding the preheated polyhexamethylene carbonate diol to the polyurethane prepolymer while stirring, and simultaneously dropping an organic bismuth catalyst, and controlling the temperature at 68-72° C. to react for 3 hours to obtain polycarbonate-modified polyurethane acrylate; The polybutadiene-modified polyurethane acrylate is prepared by the following steps: Step B1, adding hydroxy-terminated polycis-butadiene and polyether diol into a three-necked flask, vacuum dehydrating for 1 hour, adding isophorone diisocyanate, stirring and heating to 70° C. and keeping the temperature for reaction for 30 minutes, then adding a chelated tin catalyst, heating to 80° C., continuing stirring and keeping the temperature for reaction for 1.5-2 hours, to obtain a polybutadiene-modified polyurethane prepolymer; Step B2, adding 1,4-butanediol to the polybutadiene-modified polyurethane prepolymer, maintaining the temperature at 80° C. for 1 hour, then adding hydroxyethyl acrylate and a chelated tin catalyst, and performing a capping reaction for 2 hours to obtain polybutadiene-modified polyurethane acrylate.
2. An EB curing coating according to claim 1, characterized in that: The molar ratio of isophorone diisocyanate to hydroxyethyl acrylate is 1:1-1.
5.
3. An EB curing coating according to claim 1, characterized in that: The molar ratio of the polyhexamethylene carbonate diol to the polyurethane prepolymer is 1-1.5:
2.
4. An EB curing coating according to claim 1, characterized in that: The molar ratio of the terminal hydroxyl polybutadiene, polyether diol and isophorone diisocyanate is 5-8:2-5:
20.
5. An EB curing coating according to claim 1, characterized in that: The molar ratio of the polybutadiene-modified polyurethane prepolymer, 1.4-butanediol and hydroxyethyl acrylate is 2:1-2:
4.
6. An EB curing coating according to claim 1, characterized in that: The ultraviolet light absorber is hydroxyphenyl triazine; and the wetting and leveling agent is polyether-modified polydimethylsiloxane.
7. Application of an EB curing coating according to any one of claims 1 to 6 on a photovoltaic backplane PET film, characterized in that: The steps include: The EB curing coating is coated on the corona treated PET film with a wire rod, and then cured by an electron beam curing device to form a coating to obtain a photovoltaic backplane PET film.
8. The use of an EB curing coating on a photovoltaic backplane PET film according to claim 7, characterized in that: The curing voltage is 180-200 KeV, and the curing dose is 30-40 kGy.
Citation Information
Patent Citations
Synthesis method of radiation-curing polyurethane acrylate paint
CN104342015A
EB cured aluminum substrate wear-resistant coating
CN113773741A
EB-cured super-weather-resistant ink-jet gloss oil and preparation method thereof
CN114836075A
Black elastic glue based on EB curing
CN116333648A