A hexagonal chromium antimonide single crystal that can be used as an alternating magnet material, and its preparation method and application

By heating and centrifuging under high vacuum, high-quality hexagonal crystal chromium antimonide single crystals are prepared, which solves the complex problem of CrSb single crystal preparation in the prior art, and realizes high-purity and low-cost alternating magnets Material preparation.

CN118326520BActive Publication Date: 2024-11-08NINGBO UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410277956.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-12
Publication Date
2024-11-08
Estimated Expiration
2044-03-12

AI Technical Summary

Technical Problem

In the prior art, the preparation method of CrSb single crystal is complex and cumbersome, and there is a lack of a simple and effective preparation method.

Method used

Hexagonal antimony system antimony, chromium and tin were used to prepare hexagonal antimony system antimony system by centrifugation. Chromium single crystal.

Benefits of technology

The CrSb single crystal preparation with high quality, simple operation and low cost is achieved, ensuring the purity of the chromium antimonide single crystal, and the single crystal thickness is adjusted by controlling the cooling rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118326520B_ABST
    Figure CN118326520B_ABST
Patent Text Reader

Abstract

The invention discloses a hexagonal chromium antimonide single crystal that can be used as an alternating magnet material, and a preparation method and application thereof, which belongs to the field of alternating magnet materials. The preparation method provided by the invention comprises the following steps: S1: mixing metal antimony, metal chromium and metal tin in a crucible according to a molar ratio of (0.5-1.2): (0.5-1.2): (8-10), and transferring the crucible to a test tube, inserting quartz wool into the test tube, evacuating the test tube and sealing it; S2: heating the test tube to 1000°C for 480-550min and keeping it warm for 1000min, cooling it to 500°C at a cooling rate of (0.028-0.032)°C / min after the insulation is completed, and taking out the test tube; S3: removing the co-solvent to obtain a hexagonal chromium antimonide single crystal that can be used as an alternating magnet material. The preparation method of the hexagonal chromium antimonide single crystal that can be used as an alternating magnet material provided by the invention has the advantages of simple steps, low cost and high product quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of alternating magnet materials, and in particular to a hexagonal chromium antimonide single crystal that can be used as an alternating magnet material, and a preparation method and application thereof. Background Art

[0002] Alternating magnets are a recently proposed magnetic phase that is different from ferromagnetism and antiferromagnetism. Alternating magnets are similar in structure to antiferromagnetism, where the magnetic moments on different ions cancel each other out, exhibiting behavior more similar to ferromagnetism. Experiments have observed ferromagnetic phenomena in alternating magnets, such as the anomalous Hall effect, spin currents, and tunnel magnetoresistance. Therefore, alternating magnets open up new possibilities for the development of faster and more efficient storage devices, and have broad prospects for applications in spin electronics and low-dissipation nanoelectronics.

[0003] Hexagonal CrSb meets the requirements of alternating magnets in terms of symmetry, so it is listed as a candidate for alternating magnets. Therefore, preparing CrSb single crystals that meet the requirements of alternating magnet materials is the first and most important step in the research. However, the current preparation method of CrSb single crystals requires repeated grinding and annealing, which is cumbersome. Therefore, it is necessary to provide a simple method to prepare CrSb single crystals. Summary of the invention

[0004] The problem to be solved by the present invention is how to use a simpler preparation method to prepare a hexagonal chromium antimonide single crystal with a regular shape and capable of being used as an alternating magnetic material.

[0005] In order to solve the above problems, the present invention provides a method for preparing a hexagonal chromium antimonide single crystal that can be used as an alternating magnet material, comprising the following steps:

[0006] S1: Mix the raw materials in a crucible, transfer the crucible to a test tube, evacuate the test tube and seal it;

[0007] S2: heating the test tube and keeping it warm, cooling it down after the insulation is over and taking out the test tube;

[0008] S3: removing the solvent to obtain a hexagonal chromium antimonide single crystal that can be used as an alternating magnet material.

[0009] Preferably, in step S1, the raw materials are metal antimony, metal chromium, and metal tin.

[0010] Preferably, the molar ratio of the metal antimony, metal chromium and metal tin is (0.5-1.2):

[0011] (0.5~1.2):(8~10).

[0012] Preferably, the molar ratio of metal antimony, metal chromium and metal tin is 1:1:9.

[0013] Preferably, in step S1, the vacuum degree of the test tube after evacuation is less than 10 -3 Pa.

[0014] Preferably, step S2 comprises the following steps: placing the evacuated test tube in a muffle furnace, heating it to 1000° C., and keeping it at 1000° C. for 1000 min, then lowering the temperature to 500° C. and taking out the test tube.

[0015] Preferably, the heating time is 480 to 550 minutes.

[0016] Preferably, the cooling rate of the cooling is (0.028-0.032)°C / min.

[0017] Preferably, step S3 comprises the following steps: centrifuging the test tube taken out in step S2 for 40 to 120 seconds, taking out the sample in the test tube after the temperature drops to room temperature,

[0018] The flux is removed to obtain a hexagonal chromium antimonide single crystal which can be used as an alternating magnet material.

[0019] Furthermore, the second aspect of the present invention provides a hexagonal chromium antimonide single crystal that can be used as an alternating magnet material. The hexagonal chromium antimonide single crystal is a hexagonal bright single crystal with a thickness of 0.1 to 0.8 mm. The hexagonal chromium antimonide single crystal is prepared by the aforementioned preparation method.

[0020] Furthermore, the third aspect of the present invention provides an application of the aforementioned hexagonal chromium antimonide single crystal that can be used as an alternating magnet material, wherein the application is to use the hexagonal chromium antimonide single crystal as an alternating magnet material.

[0021] The present invention has the beneficial effects: in the process of controlling the temperature, the preparation method of the hexagonal chromium antimonide single crystal that can be used as an alternating magnet material provided by the present invention first raises the temperature to 1000°C, then keeps the temperature and cools it to 500°C. This process ensures the purity of the chromium antimonide single crystal. At the same time, the thickness of the hexagonal chromium antimonide single crystal is closely related to the cooling rate. The smaller the cooling rate, the greater the thickness of the hexagonal chromium antimonide single crystal finally generated. Different from the prior art, the present invention adopts a solvent method to prepare CrSb single crystals, and performs heating, cooling and centrifugation under high vacuum, wherein the solvent can be removed during the centrifugation operation, and high-quality CrSb single crystals can be prepared. The preparation method of the hexagonal chromium antimonide single crystal that can be used as an alternating magnet material provided by the present invention uses a solvent method, wherein the solvent metal used can be recycled. Compared with the prior art, the preparation method provided by the present invention has the advantages of high product quality, simple operation and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a photo of sample 1 prepared in a specific embodiment of the present invention under an optical microscope;

[0023] Figure 2 This is a refined graph of the powder XRD test spectrum of sample 1 prepared in a specific embodiment of the present invention;

[0024] Figure 3 is the EDX diffraction spectrum of sample 1 prepared in a specific embodiment of the present invention;

[0025] Figure 4 This is a comparison photo of the Laue diffraction of the sample 1 prepared in the specific embodiment of the present invention along the a-axis and the standard card;

[0026] Figure 5 is a curve diagram showing the change of magnetic susceptibility of sample 1 obtained in a specific embodiment of the present invention with temperature;

[0027] Figure 6 It is a trend diagram of the magnetic susceptibility of sample 1 prepared in a specific embodiment of the present invention changing with the magnetic field intensity. DETAILED DESCRIPTION

[0028] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. It should be noted that the following embodiments are only used to illustrate the implementation method and typical parameters of the present invention, and are not used to limit the parameter range described in the present invention. Reasonable changes derived therefrom are still within the scope of protection of the claims of the present invention.

[0029] It should be noted that the endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in this article.

[0030] Unless otherwise defined, all terms, symbols and other scientific terms used herein are intended to have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. In some cases, terms with conventionally understood meanings are defined herein for the purpose of clarification or ease of reference, and such definitions herein should not be construed as indicating significant differences from conventional understandings in the art. The technical methods described or cited herein are generally well understood by those skilled in the art and are adopted by conventional methods. Unless otherwise stated, the use of commercially available kits, reagents and instruments is carried out in accordance with the protocols and parameters given by the manufacturer.

[0031] A specific embodiment of the present invention provides a method for preparing a hexagonal chromium antimonide single crystal that can be used as an alternating magnet material, comprising the following steps:

[0032] S1: Mixing raw materials in a crucible, transferring the crucible to a test tube, inserting quartz wool into the test tube, evacuating and sealing the test tube, wherein the raw materials contain a co-solvent;

[0033] S2: heating the test tube and keeping it warm, cooling it down after the insulation is over and taking out the test tube;

[0034] S3: removing the solvent to obtain a hexagonal chromium antimonide single crystal that can be used as an alternating magnet material.

[0035] In some preferred embodiments, the raw materials include metallic antimony, metallic chromium, and metallic tin.

[0036] In some preferred embodiments, the molar ratio of metal antimony, metal chromium and metal tin is (0.5-1.2):(0.5-1.2):(8-10), wherein the molar ratio of metal antimony to metal chromium should be strictly controlled to be 1:1.

[0037] In some preferred embodiments, in step S1, the vacuum degree of the test tube after evacuation is less than 10-3Pa.

[0038] In some preferred embodiments, step S2 includes the following steps: placing the evacuated test tube in a muffle furnace, heating it to 1000° C., and keeping it at 1000° C. for 1000 min, then lowering the temperature to 500° C. and taking out the test tube.

[0039] In some preferred embodiments, the heating time is 480 to 550 minutes.

[0040] Most preferably, the heating time is 500 min.

[0041] In some preferred embodiments, the cooling rate is (0.028-0.032)°C / min.

[0042] Most preferably, the cooling rate is 0.03125°C / min.

[0043] In some preferred embodiments, step S3 includes the following steps: centrifuging the test tube taken out in step S2 for 40 to 120 seconds, taking out the sample in the test tube after the temperature drops to room temperature, removing the co-solvent, and obtaining a hexagonal chromium antimonide single crystal that can be used as an alternating magnet material.

[0044] Example 1

[0045] In a glove box, Cr:Sb:Sn raw materials were mixed in a crucible according to a molar ratio of 1:1:9, and the crucible containing the raw materials was placed in a test tube, filled with quartz wool, and then taken out of the glove box;

[0046] The taken out test tube is installed on the vacuum packaging device, and after the air inside is extracted, the sample area of ​​the test tube is burned with an oxyhydrogen machine to isolate it from the outside;

[0047] The packaged test tube was placed in a muffle furnace, and the temperature zone was set as follows: room temperature was heated to 1000°C for 500 min, kept at this temperature for 1000 min, and then cooled to 500°C at a rate of 0.03125°C / min;

[0048] Use crucible tongs to pick up the test tube that has cooled to 500℃, then quickly invert the test tube and put it into the centrifuge for centrifugation for 1 minute, and then take it out after it cools to room temperature;

[0049] After the centrifugation, the test tube was taken out and smashed open. After taking out the sample, a bright single crystal of CrSb in the shape of a hexagonal prism was observed. Some of the solvent was attached to it. After the sample was soaked in concentrated hydrochloric acid to remove the impurities on the surface, the attached Figure 1 The sample 1 shown has a thickness of 0.4 mm.

[0050] Example 2

[0051] In a glove box, Cr:Sb:Sn raw materials were mixed in a crucible at a molar ratio of 1:1:10, the crucible containing the raw materials was placed in a test tube, quartz wool was inserted into the test tube, and then taken out of the glove box;

[0052] The taken out test tube is installed on the vacuum packaging device, and after the air inside is extracted, the sample area of ​​the test tube is burned with an oxyhydrogen machine to isolate it from the outside;

[0053] The packaged test tube was placed in a muffle furnace, and the temperature zone was set as follows: room temperature was heated to 1000°C for 550 min, kept at 1000°C for 1000 min, and then cooled to 500°C at a rate of 0.03008°C / min;

[0054] Use crucible tongs to pick up the test tube that has cooled to 500℃, then quickly invert the test tube and put it into the centrifuge for centrifugation for 1 minute, and then take it out after it cools to room temperature;

[0055] The centrifuged test tube was taken out and smashed open, and the sample was taken out to observe a bright single crystal of CrSb in the shape of a hexagonal prism, on which some solvent was attached. The sample was soaked in concentrated hydrochloric acid to remove impurities on the surface, and sample 2 was obtained. The thickness of sample 2 was 0.6 mm.

[0056] Example 3

[0057] Characterization experiments

[0058] In order to evaluate the performance of the single crystal prepared by the embodiment of the present invention, sample 1 prepared in embodiment 1 was taken and subjected to powder X-ray diffraction (XRD) test, X-ray spectrometer test and vibrating sample magnetometer test.

[0059] Figure 2 Shown is the refined graph of the powder XRD test spectrum of sample 1, from which it can be seen that the performance of sample 1 is completely consistent with the theoretical results.

[0060] Figure 3 The EDX diffraction spectrum of sample 1 is shown, and the element contents are shown in the following table:

[0061] element weight atom percentage percentage Cr K 27.93 47.58 Sb 72.07 52.42 Total 100.00 100.00

[0062] It can be seen that sample 1 contains only antimony and chromium elements, and the atomic ratio of antimony to chromium meets the requirement of 1:1.

[0063] Figure 4 The following is a comparison photo of the Laue diffraction of the single crystal of sample 1 along the a-axis with the standard card. This shows that the crystal quality of sample 1 obtained after centrifugal cleaning is high, the natural cleavage plane is the ab plane, the cross section perpendicular to the c-axis is a regular hexagon or nearly a regular hexagon, and the ab axis is clearly visible.

[0064] Figure 5 The graph showing the magnetic susceptibility of sample 1 versus temperature (MT) is shown. Figure 6 The graph shows the trend of the magnetic susceptibility of sample 1 with the change of magnetic field (MH). Figure 5 and Figure 6 It can be seen that sample 1 meets the basic physical property tests such as (MT) and (MH). It can be seen that sample 1 has ferromagnetic and antiferromagnetic properties. It is not a traditional antiferromagnetic system, but an alternating magnetic system, which enriches the alternating magnetic research system.

[0065] Although the disclosure is disclosed as above, the protection scope of the disclosure is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the disclosure, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A method for preparing hexagonal chromium antimonide single crystal that can be used as an alternating magnet material, characterized in that: The following steps are involved: S1: Mixing raw materials of metal antimony, metal chromium and metal tin in a crucible, wherein the molar ratio of the metal antimony, metal chromium and metal tin is (0.5-1.2):(0.5-1.2):(8-10), and transferring the crucible to a test tube, inserting quartz wool into the test tube, evacuating the test tube and sealing it, wherein the raw materials contain a solvent; S2: Place the vacuumed test tube in a muffle furnace and heat it to 1000°C for 480-550 min. After keeping at 1000°C for 1000 min, reduce the temperature to 500°C and take out the test tube. The cooling rate is (0.028-0.032)°C / min. S3: removing the solvent to obtain a hexagonal chromium antimonide single crystal that can be used as an alternating magnet material.

2. The preparation method according to claim 1, characterized in that In step S1, the vacuum degree of the test tube after evacuation is less than 10 -3 Pa.

3. The preparation method according to claim 1, characterized in that: The step S3 comprises the following steps: centrifuging the test tube taken out in step S2, wherein the centrifugation time is 40 to 120 seconds, taking out the sample in the test tube after the temperature drops to room temperature, removing the co-solvent, and obtaining a hexagonal chromium antimonide single crystal that can be used as an alternating magnet material.

4. A hexagonal chromium antimonide single crystal that can be used as an alternating magnet material, characterized in that: The hexagonal chromium antimonide single crystal is a bright hexagonal prism-shaped single crystal with a thickness of 0.1-0.8 mm. The hexagonal chromium antimonide single crystal is prepared by the preparation method described in any one of claims 1-3.

5. An application of the hexagonal chromium antimonide single crystal as an alternating magnet material as claimed in claim 4, characterized in that: The application is to use the hexagonal chromium antimonide single crystal as an alternating magnet material.