A low-cost wear-resistant recycled PA / PET blended modified monofilament and preparation method thereof
Through the liquid phase tackification method and the use of compatible agents, the problem of difficulty in increasing the tackiness of PA and PET recycled materials in the solid phase was solved, and low-cost, wear-resistant PA/PET blended modified monofilament was prepared to meet the needs of industrial wires. Viscosity and strength requirements and suitable for a wide range of high-performance applications.
Patent Information
- Application Number
- CN202410549179.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-06
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-05-06
AI Technical Summary
The prior art is difficult to effectively integrate PA recycled materials into PET through solid-phase tackification, which cannot meet the viscosity and strength requirements of industrial wires. Especially when the viscosity-enhancing reaction temperature of PET is higher than the melting point of PA, effective tackification cannot be achieved.
By using the liquid phase tackification method, PA and PET recycled material are mixed by synthesizing different proportions of compatibilizers, and maleic anhydride-styrene copolymer and glycidyl methacrylate-styrene copolymer as compatibility agents, Liquid-phase viscosity-enhancing treatment improves viscosity and achieves full reaction of compatible agents, and meets the production of high-performance PA/PET regenerated monofilaments that meet the needs of different applications.
实现了低成本耐磨的PA/PET共混改性单丝的制备,满足工业丝的使用要求,提供了更高的韧性和强度,适用于现代农业温室工程和深海养殖网等高强度、耐 Corrosion application.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to a PA / PET blended modified monofilament and a preparation method thereof. Background Art
[0002] my country has nearly 100 million tons of renewable resources that can be recycled every year, with a value of more than 200 billion yuan, including more than 40 million tons of scrap steel, more than 30 million tons of waste paper, more than 5 million tons of scrap nonferrous metals, 6 million tons of waste plastics, more than 50 million waste tires, and more than 10 million tons of other waste materials. Compared with the use of primary resources, the use of renewable resources can save a lot of energy, water resources and production auxiliary materials. It can reduce production costs and reduce environmental pollution. This determines that the recycling of renewable resources has immeasurable value.
[0003] In the PET recycled material, PA recycled material is integrated into PET by adding a compatibilizer, thereby improving the wear resistance of the PET product. The viscosity of the PA / PET modified material obtained by simple mixing does not meet the production requirements of industrial yarns. If the solid phase thickening method is used, the thickening reaction temperature of PET is higher than the melting point of PA, and the thickening cannot be completed by the above method. In the present invention, the viscosity of the mixed modified polymer is increased by liquid phase thickening, thereby meeting the production requirements of industrial monofilaments. In addition, the required toughness and strength can be achieved by adjusting the ratio of PA to PET according to the needs of different products.
[0004] The black curtain wire made of PA / PET mixed modified monofilament is widely used in modern agricultural greenhouse projects. The black curtain wire can be used as the support wire of the vineyard. It is the best substitute for iron wire and steel wire. It can also be used in the greenhouse curtain system and outdoor awning as a film support wire.
[0005] The monofilament used in deep-sea aquaculture nets requires high strength, good flexibility, corrosion resistance, anti-aging, strong wind and wave resistance, long service life, large effective aquaculture water body, high efficiency, low comprehensive cost, low pollution, good water quality, low fish mortality rate, and good fish product quality. The PA / PET mixed modified monofilament has better toughness, high knotting strength, and is more solid and reliable. Summary of the invention
[0006] The purpose of the present invention is to provide a low-cost, wear-resistant recycled PA / PET blended modified monofilament and a preparation method thereof. By synthesizing different proportions of compatibilizers, PA and PET recycled materials in different proportions are mixed and expanded, and the use of industrial monofilaments is met by viscosity increase.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] A low-cost wear-resistant recycled PA / PET blended modified monofilament, characterized in that it comprises, by weight:
[0009] 60-80 parts of PET recycled material
[0010] PA recycled material 10-30 parts
[0011] 2-8 parts of maleic anhydride-styrene copolymer
[0012] Glycidyl methacrylate-styrene copolymer 3-10 parts
[0013] Heat stabilizer 0.3-0.8 parts
[0014] Antioxidant 0.1-0.3 parts
[0015] 1-4 parts of lubricant
[0016] The sum of the weight parts of the PET recycled material, the PA recycled material, the maleic anhydride-styrene copolymer, and the glycidyl methacrylate-styrene copolymer is 100.
[0017] The PET recycled material is a mixture of one or two of polyethylene terephthalate waste silk, recycled PET cloth strips, and PET bottle flakes in any proportion; the PA recycled material is a filler-free polycaprolactam recycled resin.
[0018] The heat stabilizer is an organic tin stabilizer; the antioxidant is one of antioxidant 1010, antioxidant 1098, and antioxidant 168, or a mixture of two or more of them in any proportion; the lubricant is one of magnesium stearate, Japanese Kao EBS (ethylene bisstearamide), and BASF Luwax EVA3, or a mixture of two or more of them in any proportion.
[0019] The organotin stabilizer is dioctyltin dilaurate or dibutyltin dilaurate.
[0020] The mass percentage of maleic anhydride in the maleic anhydride-styrene copolymer is 10-40%; the glycidyl methacrylate-styrene copolymer is prepared by free radical polymerization of glycidyl methacrylate and styrene, wherein the mass percentage of glycidyl methacrylate is 15-40%.
[0021] A method for preparing low-cost wear-resistant recycled PA / PET blended modified monofilament, characterized by comprising the following steps:
[0022] Step 1: Preparation of glycidyl methacrylate-styrene copolymer
[0023] Glycidyl methacrylate and styrene are mixed in a ratio to prepare a mixed monomer; deionized water: dispersant: emulsifier: mixed monomer: initiator are added into a three-necked flask equipped with a stirring paddle, a condenser and a thermometer in a weight ratio of 100:0.5:0.2:20:0.2, nitrogen is passed through, stirred and heated to 90°C, the reaction is continued for 8 hours, and the reaction is stopped; washing with deionized water, filtering, and drying at 80°C for 24 hours to obtain a glycidyl methacrylate-styrene copolymer;
[0024] Step 2: Preparation of PA / PET blends
[0025] The PA recycled material and the PET recycled material are dried at 80° C. for 1 hour, and stirred uniformly by a high-speed mixer according to the ratio to obtain a recycled mixed material ①; the glycidyl methacrylate-styrene copolymer, maleic anhydride-styrene copolymer, 1 / 3 of the recycled mixed material ①, a heat stabilizer, an antioxidant, and a lubricant prepared in step 1 are added to the high-speed mixer according to the ratio and uniformly mixed again to obtain a mixed material ②; the mixed material ② is added to a twin-screw extruder through a main feeder, and the remaining 2 / 3 of the recycled mixed material ① is added through a side feeder. After sufficient shearing, dispersion and mixing by the twin screw, the PA / PET blended melt is fed into a liquid phase viscosity increasing device through a booster pump, and vacuumized for reaction at a certain reaction temperature for a certain time, and then filtered through an 80-mesh filter by a melt booster pump, and then extruded, stretched, cooled, and pelletized to obtain PA / PET modified particles;
[0026] Step 3: Preparation of PA / PET blended modified monofilament
[0027] The material prepared in step 2 was dried at 135°C for 6 hours, extruded by a single screw extruder at an extrusion temperature of 275°C / 285°C / 285°C, formed by a spinneret, cooled, stretched, and heat-set to obtain a low-cost, wear-resistant PA / PET blended modified monofilament.
[0028] The dispersant in step 1 is one or more of calcium phosphate, magnesium carbonate, and calcium carbonate; the emulsifier is sodium dodecylbenzene sulfonate; the initiator is benzoyl peroxide; the mixing temperature of the high-speed mixer in step 2 is 110-120° C., the temperature of the liquid phase viscosity enhancement is 265° C., the vacuum degree requirement is: less than or equal to 20 Pa, and the reaction time is 10-15 hours.
[0029] The aspect ratio of the twin screw described in step three is 48-56:1, and the side feeding is in the sixth section of the screw; the cooling method described in step three is water cooling, and the cooling temperature is 50°C.
[0030] The stretching in step three adopts a two-stage stretching process, wherein the primary stretching temperature is 180° C. and the stretching ratio is 4 times; the secondary stretching temperature is 220° C. and the stretching ratio is 1.2 times.
[0031] The heat setting temperature in step 3 is 240°C.
[0032] The present invention selects maleic anhydride-styrene copolymer and glycidyl methacrylate-styrene copolymer as compatibilizers, wherein the maleic anhydride-styrene copolymer can react with PA resin to increase the volume, and the glycidyl methacrylate-styrene copolymer can react with PET resin to increase the volume. The maleic anhydride-styrene copolymer and the glycidyl methacrylate-styrene copolymer contain the same polystyrene segment, and maleic anhydride and glycidyl methacrylate can react. Therefore, by bridging the two copolymers, the PA resin and the PET resin can be mutually increased in volume. By adjusting the compatibilizer component and content, the compatibility modification of PA / PET recycled materials of different proportions can be adapted. Thereby expanding the volume increase range of the copolymer combination, and preparing high-performance PA / PET recycled monofilaments that meet different application requirements.
[0033] The two copolymers used in the present invention can react with the two-component resins respectively. In order to improve the compatibilizing effect of the copolymer as a compatibilizer, the two copolymers and a small amount of recycled materials are premixed first, and enter the twin screw through the main feed, and are fully mixed and dispersed in the screw to allow the compatibilizer and the recycled materials to fully react and increase the volume, and then the multi-component recycled materials are added through the side feed, thereby effectively improving the PA / PET compatibilizing effect.
[0034] The solid phase viscosity increasing reaction temperature of PET is 225-235°C, which is higher than the melting point of PA6. Therefore, PA / PET mixed modified material cannot be solid phase viscosity increased. The present invention improves the viscosity of PA / PET mixed modified material by liquid phase viscosity increasing method. Meanwhile, in the liquid phase viscosity increasing process, the compatibilizer and recycled materials of different components are fully reacted to further play the role of the compatibilizer. DETAILED DESCRIPTION
[0035] Embodiment 1:
[0036] Step 1: Preparation of glycidyl methacrylate-styrene copolymer
[0037] Glycidyl methacrylate and styrene are mixed in a ratio of 12:88 to prepare a mixed monomer. Deionized water: dispersant: emulsifier: mixed monomer: initiator are added in a weight ratio of 100:0.5:0.2:20:0.2 to a three-necked flask equipped with a stirring paddle, a condenser and a thermometer, and nitrogen is passed through. Stir and heat to 90°C, and the reaction lasts for 8 hours, and the reaction is stopped. Wash with deionized water, filter, and dry at 80°C for 24 hours to obtain a glycidyl methacrylate-styrene copolymer with a mass percentage content of 12% glycidyl methacrylate.
[0038] Step 2: Preparation of PA / PET blends
[0039] 18 parts of PA recycled material and 72 parts of PET recycled material were dried at 80°C for 1 hour, and stirred evenly in a high-speed mixer according to the proportion to obtain recycled mixed material ①. 5 parts of glycidyl methacrylate-styrene copolymer prepared in step 1, 5 parts of maleic anhydride-styrene copolymer with a maleic anhydride content of 12% by mass, 1 / 3 of recycled mixed material ①, 0.8 parts of heat stabilizer dioctyltin dilaurate, 0.3 parts of antioxidant 1098, and 3 parts of lubricant EBS were added to a high-speed mixer and mixed evenly again to obtain mixed material ②. The mixed material ② is added to the twin-screw extruder through the main feeder, and the remaining 2 / 3 of the recycled mixed material ① is added through the side feeder. After sufficient shearing, dispersion and mixing by the twin screw (length-to-diameter ratio 52:1), the temperature of the twin screw is set to 240-270°C, and the PA / PET blended melt is sent to the liquid phase viscosity increasing device through a booster pump. At a temperature of 260°C, a vacuum reaction is carried out with a vacuum degree of less than 20 Pa and a reaction time of 12 hours. The melt is then filtered through an 80-mesh filter through a melt booster pump, and then extruded, stretched, cooled, and pelletized to obtain PA / PET modified particles.
[0040] Step 3: Preparation of PA / PET blended modified monofilament
[0041] The material prepared in step 2 was dried at 135°C for 6 hours, extruded by a single screw extruder at an extrusion temperature of 275°C / 285°C / 285°C, formed by a spinneret, and water-cooled at a cooling temperature of 50°C; the primary stretching temperature was 180°C, and the stretching ratio was 4 times; the secondary stretching temperature was 220°C, and the stretching ratio was 1.2 times; the heat setting temperature was 240°C, and low-cost and wear-resistant PA / PET blended modified monofilament was obtained.
[0042] The melt index of the PA / PET mixed modified material obtained in step 2 is 18 g / 10 min (test conditions: 265° C. / 2.16 kg).
[0043] The monofilament obtained in step 3 has a diameter of 4 mm, a 1% initial tension modulus of 165 N, and a breaking strength of 4.6 cN / dtex.
[0044] Spinning condition: Occasional yarn breakage, no obvious abnormality.
[0045] Embodiment 2:
[0046] Step 1: Preparation of glycidyl methacrylate-styrene copolymer
[0047] Glycidyl methacrylate and styrene are mixed in a ratio of 25:75 to prepare a mixed monomer. Deionized water: dispersant: emulsifier: mixed monomer: initiator are added in a weight ratio of 100:0.5:0.2:20:0.2 to a three-necked flask equipped with a stirring paddle, a condenser and a thermometer, and nitrogen is passed through, stirred and heated to 90°C, and the reaction is continued for 8 hours, and the reaction is stopped. Wash with deionized water, filter, and dry at 80°C for 24 hours to obtain a glycidyl methacrylate-styrene copolymer with a mass percentage content of 25% glycidyl methacrylate.
[0048] Step 2: Preparation of PA / PET blends
[0049] 18 parts of PA recycled material and 72 parts of PET recycled material were dried at 80°C for 1 hour, and stirred evenly in a high-speed mixer according to the proportion to obtain recycled mixed material ①. 7 parts of glycidyl methacrylate-styrene copolymer prepared in step 1, 3 parts of maleic anhydride-styrene copolymer with a maleic anhydride content of 25% by mass, 1 / 3 of recycled mixed material ①, 0.8 parts of heat stabilizer dioctyltin dilaurate, 0.3 parts of antioxidant 1098, and 3 parts of lubricant EBS were added to a high-speed mixer and mixed evenly again to obtain mixed material ②. The mixed material ② is added to the twin-screw extruder through the main feeder, and the remaining 2 / 3 of the recycled mixed material ① is added through the side feeder. After sufficient shearing, dispersion and mixing by the twin screw (length-to-diameter ratio 52:1), the temperature of the twin screw is set to 240-270°C, and the PA / PET blended melt is sent to the liquid phase viscosity increasing device through a booster pump. At a temperature of 260°C, a vacuum reaction is carried out with a vacuum degree of less than 20 Pa and a reaction time of 12 hours. The melt is then filtered through an 80-mesh filter through a melt booster pump, and then extruded, stretched, cooled, and pelletized to obtain PA / PET modified particles.
[0050] Step 3: Preparation of PA / PET blended modified monofilament
[0051] The material prepared in step 2 was dried at 135°C for 6 hours, extruded by a single screw extruder at an extrusion temperature of 275°C / 285°C / 285°C, formed by a spinneret, and water-cooled at a cooling temperature of 50°C; the primary stretching temperature was 180°C, and the stretching ratio was 4 times; the secondary stretching temperature was 220°C, and the stretching ratio was 1.2 times; the heat setting temperature was 240°C, and low-cost and wear-resistant PA / PET blended modified monofilament was obtained.
[0052] The melt index of the PA / PET mixed modified material obtained in step 2 is: 19 g / 10 min (test conditions: 265° C. / 2.16 kg).
[0053] The monofilament obtained in step 3 has a diameter of 4 mm, a 1% initial tension modulus of 170 N, and a breaking strength of 4.5 cN / dtex.
[0054] Spinning condition: Occasional yarn breakage, no obvious abnormality.
[0055] Embodiment 3:
[0056] Step 1: Preparation of glycidyl methacrylate-styrene copolymer
[0057] Glycidyl methacrylate and styrene are mixed in a ratio of 40:60 to prepare a mixed monomer. Deionized water: dispersant: emulsifier: mixed monomer: initiator are added in a weight ratio of 100:0.5:0.2:20:0.2 to a three-necked flask equipped with a stirring paddle, a condenser and a thermometer, and nitrogen is passed through. Stir and heat to 90°C, and the reaction is continued for 8 hours, and the reaction is stopped. Wash with deionized water, filter, and dry at 80°C for 24 hours to obtain a glycidyl methacrylate-styrene copolymer with a mass percentage content of 40% glycidyl methacrylate.
[0058] Step 2: Preparation of PA / PET blends
[0059] 18 parts of PA recycled material and 77 parts of PET recycled material were dried at 80°C for 1 hour, and stirred evenly in a high-speed mixer according to the proportion to obtain recycled mixed material ①. 7 parts of glycidyl methacrylate-styrene copolymer prepared in step 1, 3 parts of maleic anhydride-styrene copolymer with a maleic anhydride content of 40% by mass, 1 / 3 of recycled mixed material ①, 0.8 parts of heat stabilizer dioctyltin dilaurate, 0.3 parts of antioxidant 1098, and 3 parts of lubricant EBS were added to a high-speed mixer and mixed evenly again to obtain mixed material ②. The mixed material ② is added to the twin-screw extruder through the main feeder, and the remaining 2 / 3 of the recycled mixed material ① is added through the side feeder. After sufficient shearing, dispersion and mixing by the twin screw (length-to-diameter ratio 52:1), the temperature of the twin screw is set to 240-270°C, and the PA / PET blended melt is sent to the liquid phase viscosity increasing device through a booster pump. At a temperature of 260°C, a vacuum reaction is carried out with a vacuum degree of less than 20 Pa and a reaction time of 12 hours. The melt is then filtered through an 80-mesh filter through a melt booster pump, and then extruded, stretched, cooled, and pelletized to obtain PA / PET modified particles.
[0060] Step 3: Preparation of PA / PET blended modified monofilament
[0061] The material prepared in step 2 was dried at 135°C for 6 hours, extruded by a single screw extruder at an extrusion temperature of 275°C / 285°C / 285°C, formed by a spinneret, and water-cooled at a cooling temperature of 50°C; the primary stretching temperature was 180°C, and the stretching ratio was 4 times; the secondary stretching temperature was 220°C, and the stretching ratio was 1.2 times; the heat setting temperature was 240°C, and low-cost and wear-resistant PA / PET blended modified monofilament was obtained.
[0062] The melt index of the PA / PET mixed modified material obtained in step 2 is 18g / 10min (test conditions: 265℃ / 2.16kg)
[0063] The monofilament obtained in step 3 has a diameter of 4 mm, a 1% initial tension modulus of 168 N, and a breaking strength of 4.5 cN / dtex.
[0064] Spinning condition: occasional broken yarn, no obvious abnormality
[0065] Embodiment 4:
[0066] Step 1: Preparation of glycidyl methacrylate-styrene copolymer
[0067] Glycidyl methacrylate and styrene are mixed in a ratio of 12:88 to prepare a mixed monomer. Deionized water: dispersant: emulsifier: mixed monomer: initiator are added in a weight ratio of 100:0.5:0.2:20:0.2 to a three-necked flask equipped with a stirring paddle, a condenser and a thermometer, and nitrogen is passed through. Stir and heat to 90°C, and the reaction lasts for 8 hours, and the reaction is stopped. Wash with deionized water, filter, and dry at 80°C for 24 hours to obtain a glycidyl methacrylate-styrene copolymer with a mass percentage content of 12% glycidyl methacrylate.
[0068] Step 2: Preparation of PA / PET blends
[0069] 30 parts of PA recycled material and 60 parts of PET recycled material were dried at 80°C for 1 hour, and stirred evenly in a high-speed mixer according to the proportion to obtain recycled mixed material ①. 3 parts of glycidyl methacrylate-styrene copolymer prepared in step 1, 7 parts of maleic anhydride-styrene copolymer with a maleic anhydride content of 12% by mass, 1 / 3 of recycled mixed material ①, 0.8 parts of heat stabilizer dibutyltin dilaurate, 0.1 parts of antioxidant 1010, and 4 parts of lubricant EBS were added to a high-speed mixer and mixed evenly again to obtain mixed material ②. The mixed material ② is added to the twin-screw extruder through the main feeder, and the remaining 2 / 3 of the recycled mixed material ① is added through the side feeder. After sufficient shearing, dispersion and mixing by the twin screw (length-to-diameter ratio 52:1), the temperature of the twin screw is set to 240-270°C, and the PA / PET blended melt is sent to the liquid phase viscosity increasing device through a booster pump. At a temperature of 260°C, a vacuum reaction is carried out with a vacuum degree of less than 20 Pa and a reaction time of 12 hours. The melt is then filtered through an 80-mesh filter through a melt booster pump, and then extruded, stretched, cooled, and pelletized to obtain PA / PET modified particles.
[0070] Step 3: Preparation of PA / PET blended modified monofilament
[0071] The material prepared in step 2 was dried at 135°C for 6 hours, extruded by a single screw extruder at an extrusion temperature of 275°C / 285°C / 285°C, formed by a spinneret, and water-cooled at a cooling temperature of 50°C; the primary stretching temperature was 180°C, and the stretching ratio was 4 times; the secondary stretching temperature was 220°C, and the stretching ratio was 1.2 times; the heat setting temperature was 240°C, and low-cost and wear-resistant PA / PET blended modified monofilament was obtained.
[0072] The melt index of the PA / PET mixed modified material obtained in step 2 is: 19 g / 10 min (test conditions: 265° C. / 2.16 kg).
[0073] The monofilament obtained in step 3 has a diameter of 4 mm, a 1% initial tension modulus of 150 N, and a breaking strength of 4.3 cN / dtex.
[0074] Spinning condition: Occasional yarn breakage, no obvious abnormality.
[0075] Example 5
[0076] Step 1: Preparation of glycidyl methacrylate-styrene copolymer
[0077] Glycidyl methacrylate and styrene are mixed in a ratio of 25:75 to prepare a mixed monomer. Deionized water: dispersant: emulsifier: mixed monomer: initiator are added in a weight ratio of 100:0.5:0.2:20:0.2 to a three-necked flask equipped with a stirring paddle, a condenser and a thermometer, and nitrogen is passed through, stirred and heated to 90°C, and the reaction is continued for 8 hours, and the reaction is stopped. Wash with deionized water, filter, and dry at 80°C for 24 hours to obtain a glycidyl methacrylate-styrene copolymer with a mass percentage content of 25% glycidyl methacrylate.
[0078] Step 2: Preparation of PA / PET blends
[0079] 25 parts of PA recycled material and 65 parts of PET recycled material were dried at 80°C for 1 hour, and stirred evenly using a high-speed mixer according to the ratio to obtain recycled mixed material ①. 6 parts of glycidyl methacrylate-styrene copolymer prepared in step 1, 4 parts of maleic anhydride-styrene copolymer with a maleic anhydride content of 25% by mass, 1 / 3 of recycled mixed material ①, 0.7 parts of heat stabilizer dibutyltin dilaurate, 0.2 parts of antioxidant 1010, and 3 parts of BASF EVA3 were added to a high-speed mixer and mixed evenly again to obtain mixed material ②. The mixed material ② is added to the twin-screw extruder through the main feeder, and the remaining 2 / 3 of the recycled mixed material ① is added through the side feeder. After sufficient shearing, dispersion and mixing by the twin screw (length-to-diameter ratio 52:1), the temperature of the twin screw is set to 240-270°C, and the PA / PET blended melt is sent to the liquid phase viscosity increasing device through a booster pump. At a temperature of 260°C, a vacuum reaction is carried out with a vacuum degree of less than 20 Pa and a reaction time of 12 hours. The melt is then filtered through an 80-mesh filter through a melt booster pump, and then extruded, stretched, cooled, and pelletized to obtain PA / PET modified particles.
[0080] Step 3: Preparation of PA / PET blended modified monofilament
[0081] The material prepared in step 2 was dried at 135°C for 6 hours, extruded by a single screw extruder at an extrusion temperature of 275°C / 285°C / 285°C, formed by a spinneret, and water-cooled at a cooling temperature of 50°C; the primary stretching temperature was 180°C, and the stretching ratio was 4 times; the secondary stretching temperature was 220°C, and the stretching ratio was 1.2 times; the heat setting temperature was 240°C, and low-cost and wear-resistant PA / PET blended modified monofilament was obtained.
[0082] The melt index of the PA / PET mixed modified material obtained in step 2 is: 20 g / 10 min (test conditions: 265° C. / 2.16 kg).
[0083] The monofilament obtained in step 3 has a diameter of 4 mm, a 1% initial tension modulus of 152 N, and a breaking strength of 4.4 cN / dtex.
[0084] Spinning condition: Occasional yarn breakage, no obvious abnormality.
[0085] Embodiment 6:
[0086] Step 1: Preparation of glycidyl methacrylate-styrene copolymer
[0087] Glycidyl methacrylate and styrene are mixed in a ratio of 40:60 to prepare a mixed monomer. Deionized water: dispersant: emulsifier: mixed monomer: initiator are added in a weight ratio of 100:0.5:0.2:20:0.2 to a three-necked flask equipped with a stirring paddle, a condenser and a thermometer, and nitrogen is passed through. Stir and heat to 90°C, and the reaction is continued for 8 hours, and the reaction is stopped. Wash with deionized water, filter, and dry at 80°C for 24 hours to obtain a glycidyl methacrylate-styrene copolymer with a mass percentage content of 40% glycidyl methacrylate.
[0088] Step 2: Preparation of PA / PET blends
[0089] 20 parts of PA recycled material and 70 parts of PET recycled material were dried at 80°C for 1 hour, and stirred evenly using a high-speed mixer according to the ratio to obtain recycled mixed material ①. 3 parts of glycidyl methacrylate-styrene copolymer prepared in step 1, 7 parts of maleic anhydride-styrene copolymer with a maleic anhydride content of 40% by mass, 1 / 3 of recycled mixed material ①, 0.4 parts of heat stabilizer dibutyltin dilaurate, 0.2 parts of antioxidant 1010:168=1:1, and 4 parts of BASF EVA3 were added to a high-speed mixer and mixed evenly again to obtain mixed material ②. The mixed material ② is added to the twin-screw extruder through the main feeder, and the remaining 2 / 3 of the recycled mixed material ① is added through the side feeder. After sufficient shearing, dispersion and mixing by the twin screw (length-to-diameter ratio 52:1), the temperature of the twin screw is set to 240-270°C, and the PA / PET blended melt is sent to the liquid phase viscosity increasing device through a booster pump. At a temperature of 260°C, a vacuum reaction is carried out with a vacuum degree of less than 20 Pa and a reaction time of 12 hours. The melt is then filtered through an 80-mesh filter through a melt booster pump, and then extruded, stretched, cooled, and pelletized to obtain PA / PET modified particles.
[0090] Step 3: Preparation of PA / PET blended modified monofilament
[0091] The material prepared in step 2 was dried at 135°C for 6 hours, extruded by a single screw extruder at an extrusion temperature of 275°C / 285°C / 285°C, formed by a spinneret, and water-cooled at a cooling temperature of 50°C; the primary stretching temperature was 180°C, and the stretching ratio was 4 times; the secondary stretching temperature was 220°C, and the stretching ratio was 1.2 times; the heat setting temperature was 240°C, and low-cost and wear-resistant PA / PET blended modified monofilament was obtained.
[0092] The melt index of the PA / PET mixed modified material obtained in step 2 is: 19 g / 10 min (test conditions: 265° C. / 2.16 kg).
[0093] The monofilament obtained in step 3 has a diameter of 4 mm, a 1% initial tension modulus of 143 N, and a breaking strength of 4.3 cN / dtex.
[0094] Spinning condition: Occasional yarn breakage, no obvious abnormality.
[0095] Comparative Example 1:
[0096] Step 1: Preparation of glycidyl methacrylate-styrene copolymer
[0097] Glycidyl methacrylate and styrene are mixed in a ratio of 25:75 to prepare a mixed monomer. Deionized water: dispersant: emulsifier: mixed monomer: initiator are added in a weight ratio of 100:0.5:0.2:20:0.2 to a three-necked flask equipped with a stirring paddle, a condenser and a thermometer, and nitrogen is passed through, stirred and heated to 90°C, and the reaction is continued for 8 hours, and the reaction is stopped. Wash with deionized water, filter, and dry at 80°C for 24 hours to obtain a glycidyl methacrylate-styrene copolymer with a mass percentage content of 25% glycidyl methacrylate.
[0098] Step 2: Preparation of PA / PET blends
[0099] 18 parts of PA recycled material and 72 parts of PET recycled material were dried at 80°C for 1 hour, and stirred evenly using a high-speed mixer according to the ratio to obtain a recycled mixed material ①. 7 parts of glycidyl methacrylate-styrene copolymer prepared in step 1, 3 parts of maleic anhydride-styrene copolymer with a maleic anhydride content of 20% by mass, the recycled mixed material ①, 0.8 parts of heat stabilizer dioctyltin dilaurate, 0.3 parts of antioxidant 1098, and 3 parts of lubricant EBS were added to a high-speed mixer and mixed evenly again to obtain a mixed material ②. The mixed material ② is added to the twin-screw extruder through the main feeder. After sufficient shearing, dispersion and mixing by the twin screw (length-to-diameter ratio 52:1), the temperature of the twin screw is set to 240-270°C. The PA / PET blended melt is sent to the liquid phase viscosity increasing device through a booster pump. At a temperature of 260°C, a vacuum reaction is carried out with a vacuum degree of less than 20 Pa. The reaction time is 12 hours. The melt is then filtered through an 80-mesh filter through a melt booster pump, and then extruded, stretched, cooled, and pelletized to obtain PA / PET modified particles.
[0100] Step 3: Preparation of PA / PET blended modified monofilament
[0101] The material prepared in step 2 was dried at 135°C for 6 hours, extruded by a single screw extruder at an extrusion temperature of 275°C / 285°C / 285°C, formed by a spinneret, and water-cooled at a cooling temperature of 50°C; the primary stretching temperature was 180°C, and the stretching ratio was 4 times; the secondary stretching temperature was 220°C, and the stretching ratio was 1.2 times; the heat setting temperature was 240°C, and low-cost and wear-resistant PA / PET blended modified monofilament was obtained.
[0102] The melt index of the PA / PET mixed modified material obtained in step 2 is 30 g / 10 min (test conditions: 265° C. / 2.16 kg).
[0103] The monofilament obtained in step 3 has a diameter of 4 mm, a 1% initial tension modulus of 162 N, and a breaking strength of 3.8 cN / dtex.
[0104] Spinning condition: Fiber breakage occurs occasionally, unstable
[0105] Comparative Example 2:
[0106] Step 1: Preparation of glycidyl methacrylate-styrene copolymer
[0107] Glycidyl methacrylate and styrene are mixed in a ratio of 25:75 to prepare a mixed monomer. Deionized water: dispersant: emulsifier: mixed monomer: initiator are added in a weight ratio of 100:0.5:0.2:20:0.2 to a three-necked flask equipped with a stirring paddle, a condenser and a thermometer, and nitrogen is passed through, stirred and heated to 90°C, and the reaction is continued for 8 hours, and the reaction is stopped. Wash with deionized water, filter, and dry at 80°C for 24 hours to obtain a glycidyl methacrylate-styrene copolymer with a mass percentage content of 25% glycidyl methacrylate.
[0108] Step 2: Preparation of PA / PET blends
[0109] 18 parts of PA recycled material and 72 parts of PET recycled material were dried at 80°C for 1 hour, and stirred evenly by high-speed mixer according to the ratio to obtain recycled mixed material ①. 7 parts of methacrylate glycidyl ester-styrene copolymer prepared in step 1, 3 parts of maleic anhydride-styrene copolymer with a maleic anhydride content of 20% by mass, 1 / 3 of recycled mixed material ①, 0.8 parts of thermal stabilizer dioctyltin dilaurate, 0.3 parts of antioxidant 1098, and 3 parts of lubricant EBS were added to the high-speed mixer and mixed evenly again to obtain mixed material ②. Mixed material ② was added to the twin-screw extruder through the main feeder, and the remaining 2 / 3 of recycled mixed material ① was added through the side feeder. After sufficient shearing and dispersion mixing by the twin screw (length-to-diameter ratio 52:1), the temperature of the twin screw was set to 240-270°C, and filtered through an 80-mesh filter by a melt booster pump, and then extruded, stretched, cooled, and pelletized to obtain PA / PET modified particles.
[0110] Step 3: Preparation of PA / PET blended modified monofilament
[0111] The material prepared in step 2 was dried at 135°C for 6 hours, extruded by a single screw extruder at an extrusion temperature of 275°C / 285°C / 285°C, formed by a spinneret, and water-cooled at a cooling temperature of 50°C; the primary stretching temperature was 180°C, and the stretching ratio was 4 times; the secondary stretching temperature was 220°C, and the stretching ratio was 1.2 times; the heat setting temperature was 240°C, and low-cost and wear-resistant PA / PET blended modified monofilament was obtained.
[0112] The melt index of the PA / PET mixed modified material obtained in step 2 is 42 g / 10 min (test conditions: 265° C. / 2.16 kg).
[0113] The monofilament obtained in step 3 has a diameter of 4 mm, a 1% initial tension modulus of 120 N, and a breaking strength of 2.8 cN / dtex.
[0114] Spinning condition: severe filament breakage, rough and uneven surface of single filament.
[0115] Comparative Example 3
[0116] Step 1: Preparation of glycidyl methacrylate-styrene copolymer
[0117] Glycidyl methacrylate and styrene are mixed in a ratio of 25:75 to prepare a mixed monomer. Deionized water: dispersant: emulsifier: mixed monomer: initiator are added in a weight ratio of 100:0.5:0.2:20:0.2 to a three-necked flask equipped with a stirring paddle, a condenser and a thermometer, and nitrogen is passed through, stirred and heated to 90°C, and the reaction is continued for 8 hours, and the reaction is stopped. Wash with deionized water, filter, and dry at 80°C for 24 hours to obtain a glycidyl methacrylate-styrene copolymer with a mass percentage content of 25% glycidyl methacrylate.
[0118] Step 2: Preparation of PA / PET blends
[0119] 18 parts of PA recycled material and 72 parts of PET recycled material were dried at 80°C for 1 hour, and stirred evenly using a high-speed mixer according to the ratio to obtain recycled mixed material ①. 10 parts of glycidyl methacrylate-styrene copolymer prepared in step 1, 1 / 3 of recycled mixed material ①, 0.8 parts of heat stabilizer dioctyltin dilaurate, 0.3 parts of antioxidant 1098, and 3 parts of lubricant EBS were added to the high-speed mixer and mixed evenly again to obtain mixed material ②. The mixed material ② is added to the twin-screw extruder through the main feeder, and the remaining 2 / 3 of the recycled mixed material ① is added through the side feeder. After sufficient shearing, dispersion and mixing by the twin screw (length-to-diameter ratio 52:1), the temperature of the twin screw is set to 240-270°C, and the PA / PET blended melt is sent to the liquid phase viscosity increasing device through a booster pump. At a temperature of 260°C, a vacuum reaction is carried out with a vacuum degree of less than 20 Pa and a reaction time of 12 hours. The melt is then filtered through an 80-mesh filter through a melt booster pump, and then extruded, stretched, cooled, and pelletized to obtain PA / PET modified particles.
[0120] Step 3: Preparation of PA / PET blended modified monofilament
[0121] The material prepared in step 2 was dried at 135°C for 6 hours, extruded by a single screw extruder at an extrusion temperature of 275°C / 285°C / 285°C, formed by a spinneret, and water-cooled at a cooling temperature of 50°C; the primary stretching temperature was 180°C, and the stretching ratio was 4 times; the secondary stretching temperature was 220°C, and the stretching ratio was 1.2 times; the heat setting temperature was 240°C, and low-cost and wear-resistant PA / PET blended modified monofilament was obtained.
[0122] The melt index of the PA / PET mixed modified material obtained in step 2 is 31 g / 10 min (test conditions: 265° C. / 2.16 kg).
[0123] The monofilament obtained in step 3 has a diameter of 4 mm, a 1% initial tension modulus of 135 N, and a breaking strength of 3.0 cN / dtex.
[0124] Spinning condition: Frequent yarn breakage.
[0125]
[0126] This shows the excellent technical effect of the present invention.
Claims
1. A low-cost wear-resistant recycled PA / PET blended modified monofilament, It is characterized in that The parts by weight include: 60-80 parts of PET recycled material PA recycled material 10-30 parts 2-8 parts of maleic anhydride-styrene copolymer Glycidyl methacrylate-styrene copolymer 3-10 parts Heat stabilizer 0.3-0.8 parts Antioxidant 0.1-0.3 parts 1-4 parts of lubricant The sum of the weight parts of the PET recycled material, the PA recycled material, the maleic anhydride-styrene copolymer, and the glycidyl methacrylate-styrene copolymer is 100; The mass percentage of maleic anhydride in the maleic anhydride-styrene copolymer is 10-40%; the glycidyl methacrylate-styrene copolymer is prepared by free radical polymerization of glycidyl methacrylate and styrene, wherein the mass percentage of glycidyl methacrylate is 15-40%.
2. A low-cost wear-resistant recycled PA / PET blended modified monofilament according to claim 1, It is characterized in that The PET recycled material is a mixture of one or two of polyethylene terephthalate waste silk, recycled PET cloth strips, and PET bottle flakes in any proportion; the PA recycled material is a filler-free polycaprolactam recycled resin.
3. A low-cost wear-resistant recycled PA / PET blended modified monofilament according to claim 1, It is characterized in that The heat stabilizer is an organic tin stabilizer; the antioxidant is one of antioxidant 1010, antioxidant 1098, and antioxidant 168, or a mixture of two or more of them in any proportion; the lubricant is one of magnesium stearate, Japanese Kao EBS, and BASF LuwaxEVA3, or a mixture of two or more of them in any proportion.
4. A low-cost wear-resistant recycled PA / PET blended modified monofilament according to claim 3, It is characterized in that The organotin stabilizer is dioctyltin dilaurate or dibutyltin dilaurate.
5. A method for preparing the low-cost wear-resistant recycled PA / PET blended modified monofilament according to claim 1, Features The following steps are involved: Step 1: Preparation of glycidyl methacrylate-styrene copolymer Glycidyl methacrylate and styrene are mixed in a ratio to prepare a mixed monomer; deionized water: dispersant: emulsifier: mixed monomer: initiator are added into a three-necked flask equipped with a stirring blade, a condenser and a thermometer in a weight ratio of 100:0.5:0.2:20:0.2, nitrogen is passed through, stirred and heated to 90°C, the reaction is continued for 8 hours, and the reaction is stopped; washed with deionized water, filtered, and dried at 80°C for 24 hours to obtain a glycidyl methacrylate-styrene copolymer; Step 2: Preparation of PA / PET blends The PA recycled material and the PET recycled material are dried at 80° C. for 1 hour, and stirred uniformly by a high-speed mixer according to the ratio to obtain a recycled mixed material ①; the glycidyl methacrylate-styrene copolymer, maleic anhydride-styrene copolymer, 1 / 3 of the recycled mixed material ①, a heat stabilizer, an antioxidant, and a lubricant prepared in step 1 are added to the high-speed mixer according to the ratio and uniformly mixed again to obtain a mixed material ②; the mixed material ② is added to a twin-screw extruder through a main feeder, and the remaining 2 / 3 of the recycled mixed material ① is added through a side feeder. After sufficient shearing, dispersion and mixing by the twin screw, the PA / PET blended melt is fed into a liquid phase viscosity increasing device through a booster pump, and vacuumized for reaction at a certain reaction temperature for a certain time, and then filtered through an 80-mesh filter by a melt booster pump, and then extruded, stretched, cooled, and pelletized to obtain PA / PET modified particles; Step 3: Preparation of PA / PET blended modified monofilament The material prepared in step 2 is dried at 135° C. for 6 hours, extruded by a single screw extruder at an extrusion temperature of 275° C. / 285° C. / 285° C., formed by a spinneret, cooled, stretched, and heat-set to obtain a low-cost, wear-resistant PA / PET blended modified monofilament; The dispersant in step 1 is one or more of calcium phosphate, magnesium carbonate, and calcium carbonate; the emulsifier is sodium dodecylbenzene sulfonate; the initiator is benzoyl peroxide; the mixing temperature of the high-speed mixer in step 2 is 110-120° C., the temperature of the liquid phase viscosity enhancement is 265° C., the vacuum degree requirement is: less than or equal to 20 Pa, and the reaction time is 10-15 hours; The aspect ratio of the twin screw described in step 2 is 48-56:1, and the side feeding is in the 6th section of the screw; the cooling method described in step 3 is water cooling, and the cooling temperature is 50°C.
6. A method for preparing a low-cost wear-resistant recycled PA / PET blended modified monofilament according to claim 5, It is characterized in that The stretching in step three adopts a two-stage stretching process, wherein the primary stretching temperature is 180° C. and the stretching ratio is 4 times; the secondary stretching temperature is 220° C. and the stretching ratio is 1.2 times.
7. A method for preparing a low-cost wear-resistant recycled PA / PET blended modified monofilament according to claim 5, It is characterized in that The heat setting temperature in step 3 is 240°C.