A method for preparing high-performance carbon fiber
By using low-temperature and high-temperature alternate water washing and silicone oil treatment of polyacrylonitrile spinning liquid during the preparation of carbon fiber, the existing carbon fibers are solved, and T800-grade high-performance carbon fibers are successfully prepared to meet the high-end manufacturing industry performance requirements.
Patent Information
- Application Number
- CN202410617042.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-17
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-05-17
AI Technical Summary
The existing carbon fiber preparation technology has problems such as excessive amount of wool, uneven strength and unstable quality, which is difficult to meet the demand for high-performance carbon fibers in high-end manufacturing industries.
After the polyacrylonitrile spinning liquid is sprayed, the high-performance carbon fiber is prepared by alternate treatment of low-temperature and high-temperature water washing, combined with blow-drying, oiling, high-temperature drying and steam drafting steps, which specifically include alternate water washing of cold tanks and hot tanks. Silicone oil treatment and multi-stage temperature control ensure the dense structural and mechanical properties of the fibers.
The grain orientation and structural density of carbon fibers have been significantly improved, and T800-grade high-performance carbon fibers have been obtained, with excellent mechanical properties and mechanical properties.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of carbon fiber, and in particular relates to a method for preparing high-performance carbon fiber. Background Art
[0002] Carbon fiber (CF) is a new type of fiber material with high strength and high modulus fiber with a carbon content of more than 95%. It is a microcrystalline graphite material obtained by stacking organic fibers such as flake graphite microcrystals along the axial direction of the fiber and undergoing carbonization and graphitization treatment. Carbon fiber is "soft on the outside and hard on the inside". It is lighter than metal aluminum, but stronger than steel. It also has the characteristics of corrosion resistance and high modulus. It is an important material in national defense, military industry and civilian use. It not only has the inherent intrinsic properties of carbon materials, but also has the softness and processability of textile fibers. It is a new generation of reinforcing fiber. With the continuous development of high-end manufacturing, the performance requirements for carbon fiber are getting higher and higher.
[0003] Since the beginning of the 21st century, the engineering production of T300-T800 grades has been accelerating, but the carbon fiber obtained by existing technology still has problems such as excessive amount of hair, uneven strength, and unstable quality. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention aims to provide a method for preparing high-performance carbon fiber. The preparation method comprises:
[0005] Firstly, a polyacrylonitrile spinning solution is prepared, then polyacrylonitrile precursor is prepared, and then the polyacrylonitrile precursor is carbonized to obtain high-performance carbon fiber;
[0006] The preparation method of the polyacrylonitrile precursor comprises:
[0007] After the spinning solution is spun, it first passes through an air layer and a coagulation bath in sequence to form a primary fiber, and then is first washed with low-temperature water and then washed with high-temperature water. The low-temperature water washing is set in the form of alternating cold tanks and hot tanks. The temperature of the cold tank is 40-55°C, the temperature of the hot tank is 45-60°C, and the temperature difference between the cold tank and the hot tank is 2-10°C. The temperature of the high-temperature water washing is 60-85°C, and the total water washing drafting multiple is 0.9-1.9 times;
[0008] Then, the product is blow-dried, oiled, dried at high temperature and steam-drawn to obtain polyacrylonitrile raw yarn.
[0009] Preferably, the cold tank and the hot tank are independently set at 2 to 4 levels.
[0010] Preferably, the cold tank and the hot tank are independently set to three levels.
[0011] Preferably, the spinning solution temperature is 25-40° C., the rotational viscosity is 710-750 P, the intrinsic viscosity is 1.66-1.75 dL / g, and the solid content is 18.9-19.5%.
[0012] Preferably, the air layer height is 3-5 mm; the coagulation liquid of the coagulation bath is a dimethyl sulfoxide aqueous solution with a concentration of 25%-30% and a temperature of 3-5°C.
[0013] Preferably, the oiling step is carried out in a silicone oil aqueous solution with a concentration of 2.2-3.2%; the high-temperature drying temperature is 130°C-170°C, the steam drawing steam pressure is 1.0-1.6MP, and the steam drawing multiple is 3.6-4.0 times.
[0014] Preferably, the polyacrylonitrile precursor has a fineness of 0.73-0.78 dtex, a single yarn strength of not less than 6 cN / dtex, a single yarn elongation of 10-16%, a moisture content of not more than 3%, a linear density unevenness of not more than 1.5%, a modulus of not less than 90 cN / dtex, a boiling water shrinkage of not more than 5%, and an oil content of 0.7-1.7%.
[0015] Preferably, the method for preparing polyacrylonitrile spinning solution comprises:
[0016] 12-19 parts of acrylonitrile, 0.5-1.5 parts of itaconic acid and the first solvent are dissolved at 40°C, filtered and transferred to a polymerization kettle, wherein the mass ratio of acrylonitrile to itaconic acid is 10-15:1; the mass ratio of acrylonitrile to itaconic acid to the first solvent is 1:1-2;
[0017] Then, 0.6-1.9 parts of the initiator and the second part of the solvent were dissolved at 40°C, filtered and transferred to a polymerization kettle, and the mass ratio of the initiator to the second part of the solvent was 1:14-15;
[0018] Then, a molecular weight regulator is added to carry out a polymerization reaction, wherein the mass ratio of the molecular weight regulator to acrylonitrile is 7:100;
[0019] After the reaction is completed, the polymer solution is transferred to a stripping tower through a pump to remove acrylonitrile monomer, and the absolute pressure in the stripping tower is controlled to be 0.001~0.002MPa; then it is transferred to a concentration tower for concentration, and the absolute pressure in the concentration tower is controlled to be 0.0004~0.00065MPa; then 5~10% ammonia water is added for amination for 1~2h, and then the polyacrylonitrile spinning solution is obtained after 3-stage filtration.
[0020] Preferably, the polymerization reaction is divided into two reaction stages. The first stage is carried out at 55-65° C. for 1-3 hours, and then the temperature is increased to 65-75° C. for 13-15 hours at a heating rate of 0.05-0.15° C. / min.
[0021] Preferably, the method for carbonizing polyacrylonitrile precursor comprises:
[0022] First, the carbon fiber precursor is pre-oxidized, then subjected to low-temperature carbonization and high-temperature carbonization in sequence, surface treated, washed, and then sized and dried to obtain high-performance carbon fiber.
[0023] Preferably, the pre-oxidation temperature is 230~250℃, the pre-oxidation time is 50~70 min, and the stretching ratio is 0.935~0.945 times; the low-temperature carbonization temperature is 550~650℃, and the stretching ratio is 0.92~0.94; the high-temperature carbonization temperature is 1200~1600℃, and the stretching ratio is 0.94~0.96 times; the conductivity of the surface treatment liquid is 8.3~9.0ms / cm, the total stretching ratio is 0.96~0.98 times, 0.05~0.1% silicon carbide is added to the sizing agent, the sizing agent concentration is 1.77%~1.83%, the sizing amount is 0.8~1.2%, the drying temperature is 180~220℃, and the stretching ratio is 0.996~1.004 times.
[0024] The beneficial effects of the present invention include:
[0025] In the preparation method of high-performance carbon fiber of the present invention, in the preparation process of polyacrylonitrile precursor, low-temperature water washing is set in the form of alternating cold tank and hot tank, the temperature of the cold tank is 40~55°C, and the temperature of the hot tank is 45~60°C. At 40~55°C, the grain growth rate is relatively low, which helps to "freeze" the orientation of the molecular chain. At 45~60°C, the unoriented molecular chain is further oriented. This alternating cold and hot process promotes a more uniform and orderly molecular orientation, thereby improving the grain orientation. High-temperature water washing at 60~85°C promotes the growth of grains along the preferred direction to form a denser structure. This method significantly affects the grain orientation and grain growth inside the fiber by precisely controlling the water washing temperature and the drafting multiple, thereby obtaining a precursor with a high grain orientation and a dense structure, and finally obtaining a T800-grade high-performance carbon fiber with excellent mechanical properties. DETAILED DESCRIPTION
[0026] High-performance carbon fiber specifically refers to T800 grade carbon fiber.
[0027] The present invention provides a method for preparing high-performance carbon fiber, the preparation method comprising:
[0028] Firstly, a polyacrylonitrile spinning solution is prepared, then polyacrylonitrile precursor is prepared, and then the polyacrylonitrile precursor is carbonized to obtain high-performance carbon fiber;
[0029] The preparation method of the polyacrylonitrile precursor comprises:
[0030] After the spinning solution is spun, it first passes through an air layer and a coagulation bath in sequence to form a primary fiber, and then is first washed with low-temperature water and then washed with high-temperature water. The low-temperature water washing is set in the form of alternating cold tanks and hot tanks. The temperature of the cold tank is 40-55°C, the temperature of the hot tank is 45-60°C, and the temperature difference between the cold tank and the hot tank is 2-10°C. The temperature of the high-temperature water washing is 60-85°C, and the total water washing drafting multiple is 0.9-1.9 times;
[0031] Then it is blow-dried, oiled, high-temperature dried and steam drawn in sequence to finally obtain polyacrylonitrile raw yarn.
[0032] In the preparation process of high-performance polyacrylonitrile-based carbon fibers, how to obtain high-quality polyacrylonitrile fiber precursor is the basis for preparing high-performance polyacrylonitrile-based carbon fibers, and the post-curing washing step in the precursor preparation process is particularly critical.
[0033] During the low-temperature water washing process, the polyacrylonitrile molecular chains are partially oriented under the action of temperature. The 40~55℃ in the cold tank helps to "freeze" this orientation state, and the grain growth rate is relatively low, while the slightly higher temperature in the hot tank (45~60℃) promotes further orientation of the unoriented molecular chains. This alternating cold and hot process promotes a more uniform and orderly molecular orientation, thereby improving the degree of grain orientation. By alternating water washing between a cold tank of 40~55℃ and a hot tank of 45~60℃, the raw silk undergoes slight fluctuations in temperature at the microscopic level. Although this temperature difference of 2~10℃ is relatively small, it is enough to cause local movement and rearrangement of polymer molecules, promoting moderate orientation of molecular chains.
[0034] The subsequent high-temperature water washing step (60-85°C) provides a higher energy environment, which not only further promotes the orientation of the grains, but also helps the growth of the grains. At this stage, the movement of the molecular chains is more active, which is conducive to the growth of the grains along the preferred direction and the formation of a denser structure.
[0035] In the present invention, the cold tank temperature is, for example, 40° C., 41° C., 42° C., 43° C., 44° C., 45° C., 46° C., 47° C., 48° C., 49° C., 50° C., 51° C., 52° C., 53° C., 54° C., or 55° C. The hot tank temperature is, for example, 45° C., 46° C., 47° C., 48° C., 49° C., 50° C., 51° C., 52° C., 53° C., 54° C., 55° C., 56° C., 57° C., 58° C., 59° C., or 60° C.
[0036] In the present invention, the high temperature water washing temperature is, for example, 60° C., 61° C., 62° C., 63° C., 64° C., 65° C., 66° C., 67° C., 68° C., 69° C., 70° C., 71° C., 72° C., 73° C., 74° C., 75° C., 76° C., 77° C., 78° C., 79° C., 80° C., 81° C., 82° C., 83° C., 84° C. or 85° C. The total water washing drafting multiple is, for example, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8 or 1.9 times.
[0037] Preferably, the cold tank and the hot tank are independently set at 2 to 4 levels.
[0038] In the present invention, the cold tank is, for example, set to 2 levels, 3 levels or 4 levels; the hot tank is, for example, set to 2 levels, 3 levels or 4 levels.
[0039] Specifically, the cold tank and the hot tank are arranged alternately, and the arrangement of the cold tank and the hot tank is cold tank, hot tank, cold tank, hot tank, etc. For example, the arrangement of the cold tank and the hot tank in the low-temperature water washing process is:
[0040] When the cold tank is 2 levels and the hot tank is 2 levels, the cold tank and the hot tank are arranged in the order of cold tank, hot tank, cold tank, and hot tank during the low-temperature water washing process;
[0041] When the cold tank is of level 3 and the hot tank is of level 3, the cold tank and the hot tank are arranged in sequence of cold tank, hot tank, cold tank, hot tank, cold tank and hot tank during the low-temperature water washing process;
[0042] When the cold tank is of level 4 and the hot tank is of level 4, the cold tank and the hot tank are arranged in sequence of cold tank, hot tank, cold tank, hot tank, cold tank, hot tank, cold tank, hot tank during the low-temperature water washing process;
[0043] When the cold tank is of level 3 and the hot tank is of level 2, the cold tank and the hot tank are arranged in sequence of cold tank, hot tank, cold tank, hot tank, and cold tank during the low-temperature water washing process;
[0044] When the cold tank is level 4 and the hot tank is level 3, the cold tank and the hot tank are arranged in the sequence of cold tank, hot tank, cold tank, hot tank, cold tank, hot tank and cold tank during the low-temperature water washing process.
[0045] Preferably, the cold tank and the hot tank are independently set to 3 levels, and the setting mode of the cold tank and the hot tank is cold tank, hot tank, cold tank, hot tank, cold tank, hot tank.
[0046] In a preferred embodiment of the present invention, the spinning solution temperature is 25-40° C., the rotational viscosity is 710-750 P, the intrinsic viscosity is 1.66-1.75 dL / g, and the solid content is 18.9-19.5%.
[0047] Preferably, the air layer height is 3-5 mm; the coagulation liquid of the coagulation bath is a dimethyl sulfoxide aqueous solution with a concentration of 25%-30% and a temperature of 3-5°C.
[0048] The present invention uses a dry-jet wet spinning method to prepare polyacrylonitrile precursor, that is, after the spinning solution is ejected from the spinneret hole on the spinneret, it first passes through a section of air layer (dry section) and then enters a coagulation bath to complete solidification. The height of the air layer can affect the morphology, diameter, structure and arrangement of the fiber. In the present invention, when the height of the air layer exceeds 5 mm, the fiber is stretched unevenly and the fiber breakage rate increases; when the height of the air layer is less than 3 mm, the degree of stretching is reduced when the fiber is ejected, the fiber diameter is relatively thick, and the fiber structure is relatively loose and irregularly arranged. The height of the air layer is between 3 and 5 mm, and the stretching is uniform, which is more conducive to improving the orientation and crystallinity of the fiber, making the fiber structure more compact and orderly.
[0049] The height from the air layer is, for example, 3 mm, 3.5 mm, 4 mm, 4.5 mm or 5 mm.
[0050] Preferably, the oiling step is carried out in a silicone oil aqueous solution with a concentration of 2.2-3.2%; the high-temperature drying temperature is 130°C-170°C, the steam drawing steam pressure is 1.0-1.6MP, and the steam drawing multiple is 3.6-4.0 times.
[0051] Silicone oil concentration affects the surface properties of carbon fiber, such as surface roughness, wettability and chemical reactivity, and also affects its strength, toughness and corrosion resistance.
[0052] In the present invention, the concentration of the silicone oil is, for example, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1% or 3.2%; the steam drawing steam pressure is, for example, 1.0MP, 1.1MP, 1.2MP, 1.3MP, 1.4MP, 1.5MP or 1.6MP; the steam drawing multiple is, for example, 3.6, 3.7, 3.8, 3.9 or 4.0 times.
[0053] Preferably, the polyacrylonitrile precursor has a fineness of 0.73-0.78 dtex, a single yarn strength of not less than 6 cN / dtex, a single yarn elongation of 10-16%, a moisture content of not more than 3%, a linear density unevenness of not more than 1.5%, a modulus of not less than 90 cN / dtex, a boiling water shrinkage of not more than 5%, and an oil content of 0.7-1.7%.
[0054] In a preferred embodiment of the present invention, the method for preparing polyacrylonitrile precursor is specifically as follows:
[0055] The polyacrylonitrile spinning solution at 25-40°C is transported to the spinning device through a metering pump, and is spun through a spinneret in an air layer with a height of 3-5 mm. Subsequently, the filament bundle passes through a coagulation bath of a dimethyl sulfoxide aqueous solution with a temperature of 3-5°C and a concentration of 25-30% to obtain primary fibers.
[0056] Then, the spun fiber is conveyed to a washing device through a driving roller for washing. The washing is firstly washed alternately in 2-4 stages of cold tanks at 40-55°C and 2-4 stages of hot tanks at 45-60°C. The cold tanks and hot tanks are arranged in the order of cold tank, hot tank, cold tank, hot tank..., the temperature difference between the cold and hot tanks is 2-10°C, and then a high-temperature water washing at 60-85°C is carried out. The total water washing and drawing multiples are controlled at 0.9-1.9 times.
[0057] Then, the washed fiber is air-dried and sent to the upper oil tank for oiling. The upper oil tank contains a silicone oil aqueous solution with a silicone oil concentration of 2.5-3.2%. Then, the oiled fiber is dried at 130-170°C, and the tow is sent to the steam drawing device. The steam pressure is controlled at 1.0-1.6MPa and the steam drawing multiple is controlled at 3.6-4.0 times to obtain polyacrylonitrile precursor.
[0058] In a preferred embodiment of the present invention, the method for preparing polyacrylonitrile spinning solution comprises:
[0059] 12-19 parts of acrylonitrile, 0.5-1.5 parts of itaconic acid and the first solvent are dissolved at 40°C, filtered and transferred to a polymerization kettle, wherein the mass ratio of acrylonitrile to itaconic acid is 10-15:1; the mass ratio of acrylonitrile to itaconic acid to the first solvent is 1:1-2;
[0060] Then, 0.6-1.9 parts of the initiator and the second part of the solvent were dissolved at 40°C, filtered and transferred to a polymerization kettle, and the mass ratio of the initiator to the second part of the solvent was 1:14-15;
[0061] Then, a molecular weight regulator is added to carry out a polymerization reaction, wherein the mass ratio of the molecular weight regulator to acrylonitrile is 7:100;
[0062] After the reaction is completed, the polymer solution is transferred to a stripping tower through a pump to remove acrylonitrile monomer, and the absolute pressure in the stripping tower is controlled to be 0.001~0.002MPa; then it is transferred to a concentration tower for concentration, and the absolute pressure in the concentration tower is controlled to be 0.0004~0.00065MPa; then 5~10% ammonia water is added for amination for 1~2h, and then the polyacrylonitrile spinning solution is obtained after 3-stage filtration.
[0063] Preferably, the polymerization reaction is divided into two reaction stages. The first stage is carried out at 55-65° C. for 1-3 hours, and then the temperature is increased to 65-75° C. for 13-15 hours at a heating rate of 0.05-0.15° C. / min.
[0064] The polymerization temperature directly affects the polymerization reaction conversion rate. A temperature lower than 55°C is likely to cause incomplete reaction and reduce the reaction conversion rate. A temperature higher than 75°C is likely to cause local overheating caused by too fast reaction, the generation of gel particles, increased side reactions and uneven reaction mixture, which will also reduce the reaction conversion rate. In the present invention, the temperature of the first stage polymerization kettle is, for example, 55°C, 56°C, 57°C, 58°C, 59°C, 60°C, 61°C, 62°C, 63°C, 64°C or 65°C; the temperature of the second stage polymerization kettle is, for example, 65°C, 66°C, 67°C, 68°C, 69°C, 70°C, 71°C, 72°C, 73°C, 74°C or 75°C.
[0065] In the present invention, the heating rate is, for example, 0.05°C / min, 0.06°C / min, 0.07°C / min, 0.08°C / min, 0.09°C / min, 0.1°C / min, 0.12°C / min, 0.13°C / min, 0.14°C / min or 0.15°C / min, preferably 0.09°C / min.
[0066] In the present invention, the spinning solution needs to maintain a suitable temperature range. Too low a temperature will increase the viscosity of the spinning solution, making it difficult to transport the solution through a pipeline, which will seriously affect the production efficiency. Too high a temperature may cause changes in the dimensional structure and oxidation damage to the fiber surface, reducing the performance and stability of the fiber, thereby affecting the physical properties and mechanical properties of the carbon fiber. The spinning solution temperature is, for example, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C or 40°C.
[0067] In a preferred embodiment of the present invention, the method for carbonizing polyacrylonitrile precursor comprises:
[0068] First, the carbon fiber precursor is pre-oxidized, then subjected to low-temperature carbonization and high-temperature carbonization in sequence, surface treated, washed, and then sized and dried to obtain high-performance carbon fiber.
[0069] Preferably, the pre-oxidation temperature is 230~250℃, the pre-oxidation time is 50~70 min, and the stretching ratio is 0.935~0.945 times; the low-temperature carbonization temperature is 550~650℃, and the stretching ratio is 0.92~0.94; the high-temperature carbonization temperature is 1200~1600℃, and the stretching ratio is 0.94~0.96 times; the conductivity of the surface treatment liquid is 8.3~9.0ms / cm, the total stretching ratio is 0.96~0.98 times, the sizing agent is added with a concentration of 0.05~0.1% silicon carbide, the sizing agent concentration is 1.77%~1.83%, the sizing amount is 0.8~1.2%, the drying temperature is 180~220℃, and the stretching ratio is 0.996~1.004 times.
[0070] In the present invention, the high temperature resistance, mechanical properties and electrical conductivity of carbon fiber can be enhanced by compounding silicon carbide and sizing agent, and the oxidation resistance can be increased to extend the service life of carbon fiber. The concentration of silicon carbide is, for example, 0.05%, 0.06%, 0.07%, 0.08%, 0.09% or 0.10%. The concentration of sizing agent is, for example, 0.8%, 0.9%, 1.0%, 1.1% or 1.2%.
[0071] In a preferred embodiment of the present invention, the method for carbonizing polyacrylonitrile precursor specifically comprises:
[0072] First, in a pre-oxidation furnace, in an air atmosphere, the temperature is controlled to gradually increase from 230°C to 250°C, and the yarn is kept in the pre-oxidation furnace for 50-70 minutes. The drafting ratio is 0.935-0.945 times to obtain pre-oxidized yarn.
[0073] Then, the pre-oxidized wire was sent to a low-temperature carbonization furnace. Under a nitrogen atmosphere, the temperature was controlled to gradually increase from 550°C to 650°C, and the drafting ratio was 0.92~0.94 times.
[0074] Then, it enters a high-temperature carbonization furnace, under a nitrogen atmosphere, at a temperature of 1200-1600°C and a drawing multiple of 0.94-0.96 times, to obtain carbonized wire.
[0075] Then, the carbonized wire is surface treated in an acidic medium with a conductivity of 8.3-9.0 ms / cm and then washed with water, and the total drafting ratio is 0.96-0.98 times.
[0076] Then, after sizing in a sizing agent aqueous solution with a concentration of 1.77% to 1.83%, it is dried using a steam-heated roller at a temperature of 140 to 170°C, and the sizing amount is between 0.8 and 1.2%.
[0077] Then, the sizing carbonized fiber is sequentially subjected to primary drying and secondary drying, the primary drying temperature is 180~200℃, the secondary drying temperature is 200~220℃, the drafting multiple is 0.996~1.004 times, and then it is wound into a shaft to obtain T800 grade high-performance carbon fiber.
[0078] Example 1
[0079] The specific steps for preparing high-performance carbon fiber are as follows:
[0080] (1) Preparation of polyacrylonitrile spinning solution.
[0081] 15 parts of acrylonitrile, 1 part of itaconic acid and 24 parts of dimethyl sulfoxide were dissolved at 40°C, filtered through a filter with a precision of 0.4 μm, and transferred to a polymerization kettle;
[0082] Then, 1.5 parts of azobisisobutyronitrile and 22.5 parts of dimethyl sulfoxide were dissolved at 40°C, passed through a 0.4 μm filter, and transferred to a polymerization kettle;
[0083] Then, 1.05 parts of a molecular weight regulator was added to carry out polymerization reaction.
[0084] During the polymerization reaction, multi-stage temperature control was used. In the first stage, the temperature of the polymerization kettle was controlled at 58°C. After 2 hours of reaction, the temperature was increased to 67°C at a rate of 0.09°C / min for the second stage reaction, which was kept warm for 14 hours.
[0085] After the reaction is completed, the polymer solution is transferred to a stripping tower through a pump to remove acrylonitrile monomer, and the absolute pressure in the stripping tower is controlled to be 0.002MPa; then it is transferred to a concentration tower for concentration, and the absolute pressure in the concentration tower is controlled to be 0.00065MPa; then 5% ammonia water is added for amination for 1h, and then the polyacrylonitrile spinning solution is obtained after 3-stage filtration.
[0086] The polymerization reaction conversion rate was 91.2%.
[0087] The polyacrylonitrile spinning solution has a rotational viscosity of 745P, an intrinsic viscosity of 1.84 dl / g, and a solid content of 19.28%.
[0088] (2) Preparation of polyacrylonitrile precursor
[0089] The temperature of the polyacrylonitrile spinning solution is controlled at 30°C, and is transported to the spinning device through a metering pump. The filaments are spun through a spinneret in an air layer with a height of 4 mm. Subsequently, the filament bundles pass through a coagulation bath of a dimethyl sulfoxide aqueous solution with a temperature of 4°C and a concentration of 25% to obtain primary fibers.
[0090] Then, the spun fibers are conveyed to a water washing device through a driving roller for low-temperature water washing and high-temperature water washing. The low-temperature water washing device is arranged in an alternating manner with 3 levels of 40°C cold tanks and 3 levels of 45°C hot tanks, that is, the spun fibers pass through a 40°C cold tank, a 45°C hot tank, a 40°C cold tank, a 45°C hot tank, a 40°C cold tank, and a 45°C hot tank in sequence. The temperature of the high-temperature water washing device is 85°C, and the total water washing and stretching multiple is controlled at 1.6 times.
[0091] Then, the washed fiber is blown dry by air and sent to an oiling tank for oiling. The oiling tank contains a silicone oil aqueous solution with a silicone oil concentration of 2.8%.
[0092] Then, the oiled fiber was dried at 150° C., and the filament bundle was sent to a steam drawing device, the steam pressure was controlled at 1.3 MPa, and the steam drawing ratio was 4.0 times, to obtain polyacrylonitrile precursor.
[0093] The polyacrylonitrile precursor has a fineness of 0.78 dtex, a single yarn strength of 6.9 cN / dtex, a single yarn elongation of 12%, a moisture content of 0.99%, a linear density unevenness of 1.30%, a modulus of 96 cN / dtex, a boiling water shrinkage of 4.3%, and an oil content of 1.25%.
[0094] (3) Carbonization of raw fibers
[0095] Firstly, in a pre-oxidation furnace, in an air atmosphere, the temperature is controlled to be gradually increased from 230°C to 250°C, and the fiber stays in the pre-oxidation furnace for 60 minutes with a drafting ratio of 0.92 to obtain pre-oxidized fiber.
[0096] Then, the pre-oxidized wire was sent to a low-temperature carbonization furnace, and the temperature was gradually increased from 550°C to 650°C under a nitrogen atmosphere, with a drawing ratio of 0.94 times.
[0097] Then, it enters a high-temperature carbonization furnace, under a nitrogen atmosphere, at a temperature of 1400°C and a drawing ratio of 0.95 times to obtain carbonized wire.
[0098] Then, the carbonized fibers were surface treated in an acidic medium with an electrical conductivity of 9.0 ms / cm and then washed with water, and the total drawing ratio was 0.97 times.
[0099] Then, the sheets were sized in an aqueous sizing agent solution with a concentration of 1.80%, and then dried using a steam-heated roll at 150°C. The sizing amount was 1.1%.
[0100] Then, the sizing carbonized fiber is sequentially subjected to primary drying and secondary drying, the primary drying temperature is 190°C, the secondary drying temperature is 210°C, the drafting multiple is 1, and then it is wound into a shaft to obtain T800-grade high-performance carbon fiber.
[0101] The high-performance carbon fiber obtained in Example 1 has a tensile strength of 5886 MPa, an elastic modulus of 285 GPa, an elongation at break of 2.07%, a linear density of 520 g / km, and a bulk density of 1.81 g / cm 3 , sizing agent content 1.01%.
[0102] Example 2
[0103] The specific steps for preparing high-performance carbon fiber are as follows:
[0104] (1) Preparation of polyacrylonitrile spinning solution
[0105] The steps and parameters are consistent with those in Example 1.
[0106] The polymerization reaction conversion rate was 91.2%.
[0107] The polyacrylonitrile spinning solution has a rotational viscosity of 745P, an intrinsic viscosity of 1.84 dl / g, and a solid content of 19.28%.
[0108] (2) Preparation of polyacrylonitrile precursor
[0109] The steps and parameters for preparing the primary fiber are consistent with those in Example 1.
[0110] The spun fibers are conveyed to a water washing device through a driving roller for low-temperature water washing and high-temperature water washing. The low-temperature water washing device is arranged in an alternating manner with 3 levels of 45°C cold tanks and 3 levels of 50°C hot tanks, that is, the spun fibers pass through a 45°C cold tank, a 50°C hot tank, a 45°C cold tank, a 50°C hot tank, a 45°C cold tank, and a 50°C hot tank in sequence. The temperature of the high-temperature water washing device is 85°C, and the total water washing and stretching multiple is controlled at 1.6 times.
[0111] The polyacrylonitrile precursor was obtained by oiling, drying and steam drawing, and the steps and parameters were the same as those in Example 1.
[0112] The polyacrylonitrile precursor has a fineness of 0.75 dtex, a single yarn strength of 7.7 cN / dtex, a single yarn elongation of 13%, a moisture content of 0.72%, a linear density unevenness of 1.15%, a modulus of 104 cN / dtex, a boiling water shrinkage of 3.0%, and an oil content of 0.60%.
[0113] (3) Carbonization of polyacrylonitrile precursor
[0114] The steps and parameters are consistent with those in Example 1.
[0115] The high-performance carbon fiber obtained in Example 2 has a tensile strength of 5957 MPa, an elastic modulus of 290 GPa, an elongation at break of 2.05%, a linear density of 515 g / km, and a bulk density of 1.80 g / cm 3, sizing agent content 1.04%.
[0116] Example 3
[0117] The specific steps for preparing high-performance carbon fiber are as follows:
[0118] (1) Preparation of polyacrylonitrile spinning solution
[0119] The steps and parameters are consistent with those in Example 1.
[0120] The polymerization reaction conversion rate was 91.2%.
[0121] The polyacrylonitrile spinning solution has a rotational viscosity of 745P, an intrinsic viscosity of 1.84 dl / g, and a solid content of 19.28%.
[0122] (2) Preparation of polyacrylonitrile precursor
[0123] The steps and parameters for preparing the primary fiber are consistent with those in Example 1.
[0124] The spun fibers are conveyed to a washing device through a driving roller for low-temperature washing and high-temperature washing. The low-temperature washing device is arranged in an alternating manner with 3 levels of 50°C cold tanks and 3 levels of 55°C hot tanks, that is, the spun fibers pass through a 50°C cold tank, a 55°C hot tank, a 50°C cold tank, a 55°C hot tank, a 50°C cold tank, and a 55°C hot tank in sequence. The temperature of the high-temperature washing device is 85°C, and the total washing and stretching multiple is controlled at 1.6 times.
[0125] The polyacrylonitrile precursor was obtained by oiling, drying and steam drawing, and the steps and parameters were the same as those in Example 1.
[0126] The polyacrylonitrile precursor has a fineness of 0.72 dtex, a single yarn strength of 6.1 cN / dtex, a single yarn elongation of 11.4%, a moisture content of 1.12%, a linear density unevenness of 1.40%, a modulus of 95 cN / dtex, a boiling water shrinkage of 4.6%, and an oil content of 0.80%.
[0127] (3) Carbonization of polyacrylonitrile precursor
[0128] The steps and parameters are consistent with those in Example 1.
[0129] The high-performance carbon fiber obtained in Example 3 has a tensile strength of 5874 MPa, an elastic modulus of 285 GPa, an elongation at break of 2.06%, a linear density of 519 g / km, and a bulk density of 1.80 g / cm 3 , sizing agent content is 1.12%.
[0130] Example 4
[0131] The specific steps for preparing high-performance carbon fiber are as follows:
[0132] (1) Preparation of polyacrylonitrile spinning solution
[0133] The steps and parameters are consistent with those in Example 1.
[0134] The polymerization reaction conversion rate was 91.2%.
[0135] The polyacrylonitrile spinning solution has a rotational viscosity of 745P, an intrinsic viscosity of 1.84 dl / g, and a solid content of 19.28%.
[0136] (2) Preparation of polyacrylonitrile precursor
[0137] The steps and parameters for preparing the primary fiber are consistent with those in Example 1.
[0138] The spun fibers are conveyed to a washing device through a driving roller for low-temperature washing and high-temperature washing. The low-temperature washing device is arranged in an alternating manner with 3 levels of 45°C cold tanks and 3 levels of 55°C hot tanks, that is, the spun fibers pass through a 45°C cold tank, a 55°C hot tank, a 45°C cold tank, a 55°C hot tank, a 45°C cold tank, and a 55°C hot tank in sequence. The temperature of the high-temperature washing device is 85°C, and the total washing and stretching multiple is controlled at 1.6 times.
[0139] The polyacrylonitrile precursor was obtained by oiling, drying and steam drawing, and the steps and parameters were the same as those in Example 1.
[0140] The polyacrylonitrile precursor has a fineness of 0.76 dtex, a single yarn strength of 7.4 cN / dtex, a single yarn elongation of 13.6%, a moisture content of 1.02%, a linear density unevenness of 1.30%, a modulus of 97 cN / dtex, a boiling water shrinkage of 4.0%, and an oil content of 1.09%.
[0141] (3) Carbonization of polyacrylonitrile precursor
[0142] The steps and parameters are consistent with those in Example 1.
[0143] The high-performance carbon fiber obtained in Example 4 has a tensile strength of 5796 MPa, an elastic modulus of 299 GPa, an elongation at break of 1.94%, a linear density of 502 g / km, and a bulk density of 1.79 g / cm 3 , sizing agent content 1.20%.
[0144] Example 5
[0145] The specific steps for preparing high-performance carbon fiber are as follows:
[0146] (1) Preparation of polyacrylonitrile spinning solution
[0147] The steps and parameters are consistent with those in Example 1.
[0148] The polymerization reaction conversion rate was 91.2%.
[0149] The polyacrylonitrile spinning solution has a rotational viscosity of 745P, an intrinsic viscosity of 1.84 dl / g, and a solid content of 19.28%.
[0150] (2) Preparation of polyacrylonitrile precursor
[0151] The steps and parameters for preparing the primary fiber are consistent with those in Example 1.
[0152] The spun fibers are conveyed to a washing device through a driving roller for low-temperature washing and high-temperature washing. The low-temperature washing device is arranged in an alternating manner with 3 levels of 45°C cold tanks and 3 levels of 47°C hot tanks, that is, the spun fibers pass through a 45°C cold tank, a 47°C hot tank, a 45°C cold tank, a 47°C hot tank, a 45°C cold tank, and a 47°C hot tank in sequence. The temperature of the high-temperature washing device is 85°C, and the total washing and stretching multiple is controlled at 1.6 times.
[0153] The polyacrylonitrile precursor was obtained by oiling, drying and steam drawing, and the steps and parameters were the same as those in Example 1.
[0154] The polyacrylonitrile precursor has a fineness of 0.73 dtex, a single yarn strength of 6.4 cN / dtex, a single yarn elongation of 14.2%, a moisture content of 1.37%, a linear density unevenness of 1.50%, a modulus of 91 cN / dtex, a boiling water shrinkage of 5.0%, and an oil content of 1.45%.
[0155] (3) Carbonization of polyacrylonitrile precursor
[0156] The steps and parameters are consistent with those in Example 1.
[0157] The high-performance carbon fiber obtained in Example 5 has a tensile strength of 5902 MPa, an elastic modulus of 294 GPa, an elongation at break of 2.01%, a linear density of 510 g / km, and a bulk density of 1.79 g / cm 3 , sizing agent content 0.99%.
[0158] Example 6
[0159] The specific steps for preparing high-performance carbon fiber are as follows:
[0160] (1) Preparation of polyacrylonitrile spinning solution
[0161] The steps and parameters are consistent with those in Example 1.
[0162] The polymerization reaction conversion rate was 91.2%.
[0163] The polyacrylonitrile spinning solution has a rotational viscosity of 745P, an intrinsic viscosity of 1.84 dl / g, and a solid content of 19.28%.
[0164] (2) Preparation of polyacrylonitrile precursor
[0165] The steps and parameters for preparing the primary fiber are consistent with those in Example 1.
[0166] The spun fibers are conveyed to a water washing device through a driving roller for low-temperature water washing and high-temperature water washing. The low-temperature water washing device is arranged in an alternating manner with 2 levels of 45°C cold tanks and 2 levels of 50°C hot tanks, that is, the spun fibers pass through a 45°C cold tank, a 50°C hot tank, a 45°C cold tank, and a 50°C hot tank in sequence. The temperature of the high-temperature water washing device is 85°C, and the total water washing and stretching multiple is controlled at 1.6 times.
[0167] The polyacrylonitrile precursor was obtained by oiling, drying and steam drawing, and the steps and parameters were the same as those in Example 1.
[0168] The polyacrylonitrile precursor has a fineness of 0.73 dtex, a single yarn strength of 6.7 cN / dtex, a single yarn elongation of 16%, a moisture content of 1.05%, a linear density unevenness of 1.34%, a modulus of 98 cN / dtex, a boiling water shrinkage of 3.7%, and an oil content of 0.92%.
[0169] (3) Carbonization of polyacrylonitrile precursor
[0170] The steps and parameters are consistent with those in Example 1.
[0171] The high-performance carbon fiber obtained in Example 6 has a tensile strength of 5893 MPa, an elastic modulus of 294 GPa, an elongation at break of 2.00%, a linear density of 522 g / km, and a bulk density of 1.81 g / cm 3 , sizing agent content 0.97%.
[0172] Example 7
[0173] The specific steps for preparing high-performance carbon fiber are as follows:
[0174] (1) Preparation of polyacrylonitrile spinning solution
[0175] The steps and parameters are consistent with those in Example 1.
[0176] The polymerization reaction conversion rate was 91.2%.
[0177] The polyacrylonitrile spinning solution has a rotational viscosity of 745P, an intrinsic viscosity of 1.84 dl / g, and a solid content of 19.28%.
[0178] (2) Preparation of polyacrylonitrile precursor
[0179] The steps and parameters for preparing the primary fiber are consistent with those in Example 1.
[0180] The spun fibers are conveyed to a water washing device through a driving roller for low-temperature water washing and high-temperature water washing. The low-temperature water washing device is arranged in an alternating manner with 4 levels of 45°C cold tanks and 4 levels of 50°C hot tanks, that is, the spun fibers pass through 45°C cold tank, 50°C hot tank, 45°C cold tank, 50°C hot tank, 45°C cold tank, 50°C hot tank, 45°C cold tank, and 50°C hot tank in sequence. The temperature of the high-temperature water washing device is 85°C, and the total water washing and stretching multiple is controlled at 1.6 times.
[0181] The polyacrylonitrile precursor was obtained by oiling, drying and steam drawing, and the steps and parameters were the same as those in Example 1.
[0182] The polyacrylonitrile precursor has a fineness of 0.74 dtex, a single yarn strength of 6.5 cN / dtex, a single yarn elongation of 15%, a moisture content of 0.92%, a linear density unevenness of 1.25%, a modulus of 101 cN / dtex, a boiling water shrinkage of 3.07%, and an oil content of 0.74%.
[0183] (3) Carbonization of polyacrylonitrile precursor
[0184] The same as Example 1.
[0185] The high-performance carbon fiber obtained in Example 7 has a tensile strength of 5921 MPa, an elastic modulus of 301 GPa, an elongation at break of 1.98%, a linear density of 514 g / km, and a bulk density of 1.80 g / cm 3 , sizing agent content 1.02%.
[0186] Comparative Example 1
[0187] The specific steps for preparing high-performance carbon fiber are as follows:
[0188] (1) Preparation of polyacrylonitrile spinning solution
[0189] The steps and parameters are consistent with those in Example 1.
[0190] The polymerization reaction conversion rate was 91.2%.
[0191] The polyacrylonitrile spinning solution has a rotational viscosity of 745P, an intrinsic viscosity of 1.84 dl / g, and a solid content of 19.28%.
[0192] (2) Preparation of polyacrylonitrile precursor
[0193] The steps and parameters for preparing the primary fiber are consistent with those in Example 1.
[0194] Then, the spun fiber is conveyed to a water washing device through a driving roller for low-temperature water washing and high-temperature water washing. The low-temperature water washing device is composed of 6 levels of 45°C water tanks arranged in sequence, that is, the spun fiber passes through a 45°C water tank, a 45°C water tank, a 45°C water tank, a 45°C water tank, and a 45°C water tank in sequence. The temperature of the high-temperature water washing device is 85°C, and the total water washing and stretching multiple is controlled at 1.6 times.
[0195] The polyacrylonitrile precursor was obtained by oiling, drying and steam drawing, and the steps and parameters were the same as those in Example 1.
[0196] The polyacrylonitrile precursor has a fineness of 0.75 dtex, a single yarn strength of 6.0 cN / dtex, a single yarn elongation of 15.7%, a moisture content of 1.08%, a linear density unevenness of 1.41%, a modulus of 90 cN / dtex, a boiling water shrinkage of 4.54%, and an oil content of 1.49%.
[0197] (3) Carbonization of polyacrylonitrile precursor
[0198] The steps and parameters are consistent with those in Example 1.
[0199] The high-performance carbon fiber obtained in Comparative Example 1 has a tensile strength of 5734 MPa, an elastic modulus of 295 GPa, an elongation at break of 1.94%, a linear density of 503 g / km, and a bulk density of 1.80 g / cm 3 , sizing agent content 1.03%.
[0200] Comparative Example 2
[0201] The specific steps for preparing high-performance carbon fiber are as follows:
[0202] (1) Preparation of polyacrylonitrile spinning solution
[0203] The steps and parameters are consistent with those in Example 1.
[0204] The polymerization reaction conversion rate was 91.2%.
[0205] The polyacrylonitrile spinning solution has a rotational viscosity of 745P, an intrinsic viscosity of 1.84 dl / g, and a solid content of 19.28%.
[0206] (2) Preparation of polyacrylonitrile precursor
[0207] The steps and parameters for preparing the primary fiber are consistent with those in Example 1.
[0208] Then, the spun fiber is conveyed to a water washing device through a driving roller for low-temperature water washing and high-temperature water washing. The low-temperature water washing device is composed of 6 levels of 50°C water tanks arranged in sequence, that is, the spun fiber passes through a 50°C water tank, a 50°C water tank, a 50°C water tank, a 50°C water tank, a 50°C water tank, and a 50°C water tank in sequence. The temperature of the high-temperature water washing device is 85°C, and the total water washing and stretching multiple is controlled at 1.6 times.
[0209] The polyacrylonitrile precursor was obtained by oiling, drying and steam drawing, and the steps and parameters were the same as those in Example 1.
[0210] The polyacrylonitrile precursor has a fineness of 0.72 dtex, a single yarn strength of 5.4 cN / dtex, a single yarn elongation of 15.3%, a moisture content of 1.38%, a linear density unevenness of 1.46%, a modulus of 91 cN / dtex, a boiling water shrinkage of 4.37%, and an oil content of 1.51%.
[0211] (3) Carbonization of polyacrylonitrile precursor
[0212] The steps and parameters are consistent with those in Example 1.
[0213] The high-performance carbon fiber obtained in Comparative Example 2 has a tensile strength of 5908 MPa, an elastic modulus of 298 GPa, an elongation at break of 1.98%, a linear density of 511 g / km, and a bulk density of 1.79 g / cm 3 , sizing agent content 1.15%.
[0214] Comparative Example 3
[0215] The specific steps for preparing high-performance carbon fiber are as follows:
[0216] (1) Preparation of polyacrylonitrile spinning solution
[0217] The steps and parameters are consistent with those in Example 1.
[0218] The polymerization reaction conversion rate was 91.2%.
[0219] The polyacrylonitrile spinning solution has a rotational viscosity of 745P, an intrinsic viscosity of 1.84 dl / g, and a solid content of 19.28%.
[0220] (2) Preparation of polyacrylonitrile precursor
[0221] The steps and parameters for preparing the primary fiber are consistent with those in Example 1.
[0222] The spun fibers are conveyed to a water washing device through a driving roller for low-temperature water washing and high-temperature water washing. The low-temperature water washing device comprises three levels of 45°C water tanks and three levels of 50°C water tanks arranged in sequence, that is, the spun fibers pass through a 45°C cold tank, a 45°C cold tank, a 45°C cold tank, a 50°C hot tank, a 50°C hot tank, and a 50°C hot tank in sequence. The temperature of the high-temperature water washing device is 85°C, and the total water washing and stretching multiple is controlled at 1.6 times.
[0223] The polyacrylonitrile precursor was obtained by oiling, drying and steam drawing, and the steps and parameters were the same as those in Example 1.
[0224] The polyacrylonitrile precursor has a fineness of 0.76 dtex, a single yarn strength of 5.0 cN / dtex, a single yarn elongation of 13.4%, a moisture content of 1.29%, a linear density unevenness of 1.50%, a modulus of 89 cN / dtex, a boiling water shrinkage of 4.91%, and an oil content of 1.54%.
[0225] (3) Carbonization of polyacrylonitrile precursor
[0226] The steps and parameters are consistent with those in Example 1.
[0227] The high-performance carbon fiber obtained in Comparative Example 3 has a tensile strength of 5793 MPa, an elastic modulus of 302 GPa, an elongation at break of 1.92%, a linear density of 501 g / km, and a bulk density of 1.79 g / cm 3 , sizing agent content 1.08%.
[0228] Comparative Example 4
[0229] The specific steps for preparing high-performance carbon fiber are as follows:
[0230] (1) Preparation of polyacrylonitrile spinning solution
[0231] The steps and parameters are consistent with those in Example 1.
[0232] The polymerization reaction conversion rate was 91.2%.
[0233] The polyacrylonitrile spinning solution has a rotational viscosity of 745P, an intrinsic viscosity of 1.84 dl / g, and a solid content of 19.28%.
[0234] (2) Preparation of polyacrylonitrile precursor
[0235] The steps and parameters for preparing the primary fiber are consistent with those in Example 1.
[0236] The spun fibers are conveyed to a water washing device through a driving roller for low-temperature water washing and high-temperature water washing. The low-temperature water washing device is arranged in an alternating manner with 3 levels of 30°C cold tanks and 3 levels of 50°C hot tanks, that is, the spun fibers pass through a 30°C cold tank, a 50°C hot tank, a 30°C cold tank, a 50°C hot tank, a 30°C cold tank, and a 50°C hot tank in sequence. The temperature of the high-temperature water washing device is 85°C, and the total water washing and stretching multiple is controlled at 1.6 times.
[0237] The polyacrylonitrile precursor was obtained by oiling, drying and steam drawing, and the steps and parameters were the same as those in Example 1.
[0238] The polyacrylonitrile precursor has a fineness of 0.79 dtex, a single yarn strength of 6.2 cN / dtex, a single yarn elongation of 11.2%, a moisture content of 1.05%, a linear density unevenness of 1.33%, a modulus of 88 cN / dtex, a boiling water shrinkage of 3.8%, and an oil content of 0.9%.
[0239] (3) Carbonization of polyacrylonitrile precursor
[0240] The steps and parameters are consistent with those in Example 1.
[0241] The high-performance carbon fiber obtained in Comparative Example 4 has a tensile strength of 5764 MPa, an elastic modulus of 284 GPa, an elongation at break of 2.03%, a linear density of 523 g / km, and a bulk density of 1.81 g / cm 3 , sizing agent content 1.10%.
[0242] Comparative Example 5
[0243] The specific steps for preparing high-performance carbon fiber are as follows:
[0244] (1) Preparation of polyacrylonitrile spinning solution
[0245] The steps and parameters are consistent with those in Example 1.
[0246] 5793 MPa, elastic modulus 302 GPa, elongation at break 1.92%, linear density 501 g / km, bulk density 1.79 g / cm 3 , sizing agent content 1.08%.
[0247] (2) Preparation of polyacrylonitrile precursor
[0248] The steps and parameters for preparing the primary fiber are consistent with those in Example 1.
[0249] The spun fibers are conveyed to a water washing device through a driving roller for low-temperature water washing and high-temperature water washing. The low-temperature water washing device is arranged in an alternating manner with 3 levels of 45°C cold tanks and 3 levels of 70°C hot tanks, that is, the spun fibers pass through a 45°C cold tank, a 70°C hot tank, a 45°C cold tank, a 70°C hot tank, a 45°C cold tank, and a 70°C hot tank in sequence. The temperature of the high-temperature water washing device is 85°C, and the total water washing and stretching multiple is controlled at 1.6 times.
[0250] The polyacrylonitrile precursor was obtained by oiling, drying and steam drawing, and the steps and parameters were the same as those in Example 1.
[0251] The polyacrylonitrile precursor has a fineness of 0.73 dtex, a single yarn strength of 5.4 cN / dtex, a single yarn elongation of 14.3%, a moisture content of 1.42%, a linear density unevenness of 1.37%, a modulus of 94 cN / dtex, a boiling water shrinkage of 4.2%, and an oil content of 1.45%.
[0252] (3) Carbonization of polyacrylonitrile precursor
[0253] The steps and parameters are consistent with those in Example 1.
[0254] The high-performance carbon fiber obtained in Comparative Example 5 has a tensile strength of 5900 MPa, an elastic modulus of 299 GPa, an elongation at break of 1.97%, a linear density of 518 g / km, and a bulk density of 1.80 g / cm 3 , sizing agent content 1.03%.
Claims
1. A method for preparing high-performance carbon fiber, It is characterized in that The preparation method comprises: Firstly, a polyacrylonitrile spinning solution is prepared, then a polyacrylonitrile precursor is prepared, and then the polyacrylonitrile precursor is carbonized to obtain a high-performance carbon fiber; The preparation method of the polyacrylonitrile precursor comprises: After the spinning solution is spun, it first passes through an air layer and a coagulation bath in sequence to form a primary fiber, and then is first washed with low-temperature water and then washed with high-temperature water. The low-temperature water washing is set in the form of alternating cold tanks and hot tanks. The temperature of the cold tank is 40-55°C, the temperature of the hot tank is 45-60°C, and the temperature difference between the cold tank and the hot tank is 2-10°C. The temperature of the high-temperature water washing is 60-85°C, and the total water washing drafting multiple is 0.9-1.9 times; Then, the raw polyacrylonitrile yarn is obtained by drying, oiling, high temperature drying and steam drawing in sequence; The air layer height is 3-5 mm; the coagulation liquid of the coagulation bath is a dimethyl sulfoxide aqueous solution with a concentration of 25%-30% and a temperature of 3-5°C; The method for preparing polyacrylonitrile spinning solution comprises: 12-19 parts of acrylonitrile, 0.5-1.5 parts of itaconic acid and the first solvent are dissolved at 40°C, filtered and transferred to a polymerization kettle, wherein the mass ratio of acrylonitrile to itaconic acid is 10-15:1; the mass ratio of acrylonitrile to itaconic acid to the first solvent is 1:1-2; Then, 0.6-1.9 parts of the initiator and the second part of the solvent were dissolved at 40°C, filtered and transferred to a polymerization kettle, and the mass ratio of the initiator to the second part of the solvent was 1:14-15; Then, a molecular weight regulator is added to carry out a polymerization reaction, wherein the mass ratio of the molecular weight regulator to acrylonitrile is 7:100; The polymerization reaction is divided into two reaction stages. The first stage is a reaction at 55-65°C for 1-3 hours, and then the temperature is increased to 65-75°C at a heating rate of 0.05-0.15°C / min for a second stage for a reaction at 13-15 hours. After the reaction is completed, the polymer solution is transferred to a stripping tower through a pump to remove acrylonitrile monomer, and the absolute pressure in the stripping tower is controlled to be 0.001~0.002MPa; then it is transferred to a concentration tower for concentration, and the absolute pressure in the concentration tower is controlled to be 0.0004~0.00065MPa; then 5~10% ammonia water is added for amination for 1~2h, and then the polyacrylonitrile spinning solution is obtained after 3-stage filtration.
2. The preparation method according to claim 1, It is characterized in that The cold tank and the hot tank are independently set at 2 to 4 levels.
3. The preparation method according to claim 1, It is characterized in that The spinning solution has a temperature of 25-40° C., a rotational viscosity of 710-750P, an intrinsic viscosity of 1.66-1.75 dL / g, and a solid content of 18.9-19.5%.
4. The preparation method according to claim 1, It is characterized in that The oiling step is carried out in a silicone oil aqueous solution with a concentration of 2.2-3.2%; the high-temperature drying temperature is 130°C-170°C, the steam drawing steam pressure is 1.0-1.6MP, and the steam drawing multiple is 3.6-4.0 times.
5. The preparation method according to claim 1, It is characterized in that The polyacrylonitrile raw yarn has a fineness of 0.73-0.78 dtex, a single yarn strength of not less than 6 cN / dtex, a single yarn elongation of 10-16%, a moisture content of not more than 3%, a linear density unevenness of not more than 1.5%, a modulus of not less than 90 cN / dtex, a boiling water shrinkage of not more than 5%, and an oil content of 0.7-1.7%.
6. The preparation method according to claim 1, It is characterized in that The method of carbonizing polyacrylonitrile precursor includes: First, the carbon fiber precursor is pre-oxidized, then subjected to low-temperature carbonization and high-temperature carbonization in sequence, surface treated, washed, and then sized and dried to obtain high-performance carbon fiber.
7. The preparation method according to claim 6, It is characterized in that The pre-oxidation temperature is 230-250° C., the pre-oxidation time is 50-70 min, and the drafting ratio is 0.935-0.945 times; the low-temperature carbonization temperature is 550-650° C., and the drafting ratio is 0.92-0.94; the high-temperature carbonization temperature is 1200-1600° C., and the drafting ratio is 0.94-0.96 times; the conductivity of the surface treatment liquid is 8.3-9.0 ms / cm, the total drafting ratio is 0.96-0.98 times, 0.05-0.1% silicon carbide is added to the sizing agent, the sizing agent concentration is 1.77%-1.83%, the sizing amount is 0.8-1.2%, the drying temperature is 180-220° C., and the drafting ratio is 0.996-1.004 times.