A piezoelectric stack structure and manufacturing method
By utilizing the residual stress of the piezoelectric layer in the piezoelectric laminated structure to bend the structural layer toward the direction of the piezoelectric layer and adjusting the PECVD process parameters, the problem of difficulty in controlling the direction of disturbance in traditional technology is solved, and the piezoelectric laminated structure is realized. negative interference and high performance.
Patent Information
- Application Number
- CN202410481187.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-22
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-04-22
AI Technical Summary
The residual stress generated in the traditional piezoelectric stacked structure during high-temperature processes causes disturbance, making it difficult to achieve bending deformation in the direction of the piezoelectric layer and affecting device performance.
By arranging a disturbance limiting layer, a piezoelectric layer and a structural layer on the substrate, the residual stress of the piezoelectric layer is used to bend the structural layer toward the piezoelectric layer, and the PECVD process parameters are adjusted to control the direction and size of the stress to make the laminated structure The initial disturbance of is negative, ensuring that the residual stress and vibration stress are superimposed.
It achieves the negative interference of the piezoelectric stack structure, improves the sensitivity and performance of the device, ensures stress superposition in the effective working area, and increases the vibration amplitude of the diaphragm.
Smart Images

Figure CN118338759B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of piezoelectric stacked structures and manufacturing technology in semiconductor processes, and in particular to a piezoelectric stacked structure and a manufacturing method. Background Art
[0002] At present, as the core of piezoelectric MEMS sensors, piezoelectric stack structures often have residual stress caused by the difference in thermal expansion coefficients of each layer of material. These residual stresses caused by high-temperature processes will cause the piezoelectric stack structure to deform and bend in a certain direction. After the piezoelectric stack structure is bent, the position of the cross section of the stack structure will change. The displacement of the cross section perpendicular to the axial direction of the stack structure is called deflection. Figure 1 shown.
[0003] Generally, during the design and processing of piezoelectric MEMS sensors, it is hoped that the piezoelectric stacked structure is sufficiently flat, that is, extremely low positive or negative disturbance. However, due to the objective existence of the difference in thermal expansion coefficients of the stacked structure, the stacked structure must have a certain amount of disturbance. Although the disturbance of the piezoelectric stacked structure is undesirable in most MEMS devices. However, in vibration detection piezoelectric MEMS sensors, such as microphones, ultrasonic sensors, and sonic vibration sensors, the disturbance of the stacked structure can be utilized. Figure 2 As shown in the figure, the disturbance caused by the residual stress Se is parabolic, while the contribution of the stress Sb generated by the vibration on the laminated structure to the disturbance is approximately linear. Therefore, the combined stress S after superposition is the result of Se and Sb superimposing each other on the negative disturbance side, while Se and Sb cancel each other out on the positive disturbance side. Therefore, in engineering, it is hoped that the final disturbance of the piezoelectric laminate is in the interval where the residual stress and vibration stress are superimposed and increased.
[0004] In the piezoelectric stack structure, the thickness of the structural layer is often several to dozens of times thicker than the piezoelectric layer, so the neutral plane of the piezoelectric stack is located in the structural layer. The braking mechanism of piezoelectric vibration shows that the neutral plane to the piezoelectric layer is the effective working area of the piezoelectric stack. Since in actual situations, the piezoelectric stack will have initial disturbances, different disturbances will have different effects on the piezoelectric stack. When the disturbance direction is toward the piezoelectric layer, that is, one side of the piezoelectric layer bulges outward, the residual stress and vibration stress in the neutral plane to the piezoelectric layer area are superimposed, while the stress from the neutral plane to the structural layer is offset. At this time, the stress in the effective working area of the piezoelectric stack is superimposed, and the diaphragm can produce higher sensitivity, which is beneficial to the improvement of device performance. When the disturbance direction of the piezoelectric stack is toward the structural layer, that is, one side of the structural layer bulges outward, the stress situation is just the opposite, which is not conducive to the improvement of device performance.
[0005] Among the many piezoelectric materials, lead zirconate titanate (PZT) piezoelectric material can be grown on a substrate through a magnetron sputtering process to obtain a PZT piezoelectric film with high film quality, high piezoelectric coefficient, high stability and reliability. However, the growth process of the PZT film will produce a large residual stress. This residual stress manifests as a tensile stress and is much larger than the initial disturbance of the substrate. For traditional substrates based on silicon wafers or SOI wafers, after the growth of the PZT thin film layer (piezoelectric layer) is completed, the stacked structure has a large negative disturbance, that is, the disturbance direction of the piezoelectric stack is in the direction of the structural layer (such as Figure 3 As shown in A). Therefore, it is difficult to obtain a piezoelectric stack with the disturbance direction toward the piezoelectric layer using conventional process methods.
[0006] In summary, the present invention proposes a piezoelectric stack structure and a manufacturing method thereof to solve the above-mentioned problems. Summary of the invention
[0007] The purpose of the present invention is to solve the problems raised in the background technology, propose a piezoelectric stack structure and its manufacturing process, utilize the negative disturbance brought by the residual stress of the piezoelectric layer, make the structural layer grown on the surface of the piezoelectric layer bend and deform toward the piezoelectric layer, make the disturbance of the piezoelectric stack structure negative disturbance, make the residual stress and vibration stress in the effective working area superimpose, and improve the performance of the device.
[0008] Embodiments of the present invention provide a piezoelectric stack structure and a manufacturing method.
[0009] The first aspect: A piezoelectric stack structure includes a substrate, the substrate has a relative front and back side, and is characterized in that it also includes a disturbance limiting layer, a piezoelectric layer and a structural layer stacked in sequence on the front side of the substrate, the piezoelectric layer bends and deforms toward the substrate, and the structural layer bends and deforms toward the piezoelectric layer, so that the initial disturbance of the piezoelectric stack structure is in a negative direction, and the residual stress and vibration stress in the effective working area of the piezoelectric stack structure are superimposed.
[0010] As a further solution of the present invention, a back cavity is opened on the back side of the substrate.
[0011] As a further solution of the present invention, the substrate is a silicon wafer substrate.
[0012] As a further solution of the present invention, the piezoelectric layer includes a PZT lower electrode, a PZT film and a PZT upper electrode which are stacked in sequence, and the disturbance direction of the PZT film is a negative direction.
[0013] As a further solution of the present invention, the thickness of the PZT film is 0.1-5 μm.
[0014] As a further solution of the present invention, the thickness of the structural layer is greater than the thickness of the PZT film.
[0015] As a further solution of the present invention, metal layers are grown on the surfaces of the PZT lower electrode and the PZT upper electrode respectively to facilitate leading out the electrodes.
[0016] As a further solution of the present invention, the longitudinal projection area of the PZT upper electrode is smaller than the longitudinal projection area of the PZT film, and the structural layer is arranged on the surface of the PZT upper electrode and extends to the surface of the PZT film.
[0017] As a further solution of the present invention, the material of the perturbation limiting layer is silicon oxide, and the thickness of the perturbation limiting layer is 10-500 nm.
[0018] As a further solution of the present invention, the material of the structural layer is silicon oxide and / or silicon nitride, and the thickness of the structural layer is 0.5-25 μm.
[0019] As a further solution of the present invention, the structural layer is a double-layer structure or a triple-layer structure in which silicon oxide and silicon nitride are alternately stacked in sequence.
[0020] A second aspect: A method for manufacturing a piezoelectric stack, comprising the steps of:
[0021] S1. A disturbance limiting layer is grown on the front side of the substrate by a thermal oxidation process;
[0022] S2, sputtering and growing a piezoelectric layer on the disturbance limiting layer, the piezoelectric layer bends and deforms toward the substrate due to its own stress;
[0023] S3, patterning the piezoelectric layer;
[0024] S4, growing a structural layer on the patterned piezoelectric layer, wherein the structural layer is bent and deformed toward the piezoelectric layer;
[0025] S5, graphing the structural layer;
[0026] S6, etching the back side of the substrate to form a back cavity;
[0027] The piezoelectric layer bends and deforms toward the substrate, and the structural layer bends and deforms toward the piezoelectric layer, so that the initial disturbance of the piezoelectric stack structure is in the negative direction, and the residual stress and vibration stress in the effective working area of the piezoelectric stack structure are superimposed.
[0028] As a further solution of the manufacturing method of the present invention, the step of sputtering and growing a piezoelectric layer on the disturbance limiting layer in S2 includes:
[0029] S21, sputtering and growing a layer of PZT lower electrode on the disturbance limiting layer;
[0030] S22, sputtering a PZT film on the PZT lower electrode, and the PZT film bends and deforms toward the PZT lower electrode due to its own stress;
[0031] S23. A layer of PZT upper electrode is sputtered and grown on the PZT film, and the PZT upper electrode is bent and deformed along the bending direction of the PZT film.
[0032] As a further solution of the manufacturing method of the present invention, the piezoelectric layer is patterned in S3, including:
[0033] S31, etching the PZT upper electrode by IBE to pattern the PZT upper electrode;
[0034] S32, wet etching the PZT film to expose a portion of the PZT lower electrode;
[0035] S33, etching the PZT lower electrode by IBE to pattern the PZT lower electrode, thereby completing the patterning of the piezoelectric layer.
[0036] As a further solution of the manufacturing method of the present invention, it also includes:
[0037] S34, growing a metal layer on the surface of the piezoelectric layer, wherein the metal layer covers exposed areas of the piezoelectric layer and the interference limiting layer;
[0038] S35, patterning the metal layer, retaining a portion of the metal layer on the surface of the PZT lower electrode and the PZT upper electrode.
[0039] As a further solution of the manufacturing method of the present invention, the structural layer is generated by a low-temperature PECVD process, and the structural layer is a double-layer structure or a three-layer structure in which silicon oxide and silicon nitride are alternately stacked in sequence.
[0040] As a further solution of the manufacturing method of the present invention, the stress direction and magnitude of the structural layer are controlled by adjusting the temperature, time, power and chamber pressure of the low-temperature PECVD process.
[0041] Beneficial effects of the present invention:
[0042] 1. The present invention arranges a structural layer on the piezoelectric layer through the PECVD process. The piezoelectric layer is deformed and bent downward due to its own stress. The stress direction and size of the structural layer are adjusted by adjusting the process parameters of PECVD to achieve the purpose of deformation and deflection of the structural layer toward the piezoelectric layer. The structural disturbances of each layer from the neutral plane of the laminated structure to the piezoelectric layer in the present invention are all in the negative direction. The residual stress and vibration stress in the effective working area are superimposed, and the vibration amplitude of the diaphragm is increased, which can produce higher sensitivity during detection and improve device performance.
[0043] 2. The structural layer of the present invention adopts three material layers. The middle layer plays the main role of controlling the neutral surface. The main function of the bottom layer is to improve the adhesion of the middle layer and improve the film quality. The main function of the top layer is to enhance the tensile strength of the middle layer and improve the stability of the entire structural layer. The three-layer structure is more stable and reliable, and the yield rate is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 Schematic diagram of the disturbance generated by the piezoelectric stack;
[0045] Figure 2 It is a schematic diagram of the residual stress, vibration stress and combined stress of the piezoelectric stack;
[0046] Figure 3 It is a schematic diagram of a structure in which a piezoelectric stack structure bulges toward a structural layer and a piezoelectric stack structure bulges toward a piezoelectric layer;
[0047] Figure 4 It is a schematic diagram of the piezoelectric stack structure of the present invention;
[0048] Figure 5 It is a schematic diagram of the piezoelectric stack separation structure of the present invention;
[0049] Figure 6 for Figure 5 A schematic structural diagram of one embodiment of the present invention;
[0050] Figure 7 For the present invention Figure 5 sectional view of
[0051] Figure 8 For the present invention Figure 6 sectional view of
[0052] Fig. 9 It is a schematic diagram of the structural layer in the preferred embodiment of the present invention;
[0053] Figure 10-12 They are schematic diagrams of structural layers in various embodiments of the present invention;
[0054] Figure 13-Figure 18 for Figure 5 Schematic diagram of the process flow;
[0055] Fig.13 , Fig.14 , Figure 19-22 for Figure 6 Schematic diagram of the process flow.
[0056] In the accompanying drawings: 1, piezoelectric layer; 11, PZT lower electrode; 12, PZT thin film; 13, PZT upper electrode; 2, structural layer; 3, substrate; 4, disturbance limiting layer; 5, metal layer. DETAILED DESCRIPTION
[0057] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar symbols throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0058] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in conjunction with specific embodiments.
[0059] Embodiment 1:
[0060] like Figure 4 , Figure 5 and Figure 7 As shown, the piezoelectric stack structure proposed in an embodiment of the present invention includes a substrate 3, a disturbance limiting layer 4, a piezoelectric layer 1 and a structural layer 2 which are stacked in sequence, a back cavity is opened at the bottom of the substrate 3, and the areas of the disturbance limiting layer 4, the piezoelectric layer 1 and the structural layer 2 on the longitudinal projection area of the back cavity jointly form a diaphragm.
[0061] The piezoelectric layer 1 in the embodiment of the present invention will be deformed and bent downward due to stress after growth. The structural layer 2 is formed on the surface of the piezoelectric layer 1 through the PECVD process. By adjusting the parameters of the PECVD process, the stress direction and magnitude of the structural layer 2 are adjusted, so that the structural layer 2 is deformed and bent toward the piezoelectric layer 1. The structural disturbances of each layer from the neutral plane to the piezoelectric layer are all in the negative direction. The residual stress and vibration stress in the effective working area are added, which can produce higher sensitivity during detection and improve device performance.
[0062] Optionally, the substrate 3 is made of a silicon wafer, the disturbance of which is substantially zero, which is beneficial to reducing the influence of the substrate 3 on the disturbance of each layer during the production process.
[0063] like Figure 4 and Figure 5 As shown, the perturbation limiting layer 4 can be grown on the front side of the silicon wafer using a thermal oxidation growth process to form the perturbation limiting layer 4; the stress of the silicon oxide grown by thermal oxidation will cause the perturbation limiting layer 4 to produce negative perturbations, but the thickness of the perturbation limiting layer 4 is much smaller than the substrate 3, so the perturbation limiting layer 4 has no effect on the perturbations of the entire stacked structure. At the same time, since the silicon oxide grown by the thermal oxidation process has a higher density and a higher Young's modulus, based on the interface effect, the perturbation limiting layer 4 limits the perturbation of the piezoelectric layer 1 from being too large during the growth process, thereby avoiding adverse effects. Optionally, the thickness of the perturbation limiting layer 4 is 10-500nm.
[0064] like Figure 6 , Figure 7 and Figure 8As shown, the piezoelectric layer 1 is formed on the surface of the disturbance limiting layer 4, and the piezoelectric layer 1 includes a stacked PZT lower electrode 11, a PZT film 12 and a PZT upper electrode 13, wherein the disturbance direction of the PZT film 12 is the negative direction.
[0065] Optionally, the material of the PZT upper electrode 13 and the PZT lower electrode 11 is a buffer layer formed by metals such as Pt, Au, Ti, and metal compounds; optionally, the thickness of the PZT film 12 is 0.1-5 μm.
[0066] Due to the effect of the perturbation limiting layer 4, the perturbation of the PZT film 12 will be affected by the thickness of the PZT film 12, that is, PZT films 12 of different thicknesses will cause different perturbations of the piezoelectric stack structure. Since the growth process of the PZT film 12 will cause the PZT film 12 to produce a large tensile stress, the PZT film 12 that has been grown has a perturbation in the negative direction, causing the piezoelectric stack structure to bend downward as a whole. With the combined effect of the perturbation limiting layer 4 and the control of the growth process parameters of the PZT film 12, the perturbation of the PZT film 12 will be controlled in an appropriate orientation, which can avoid reliability problems such as local stress concentration, abnormal electric domain distribution, mechanical fatigue, and material nonlinearity in the PZT film 12; at the same time, it will also avoid excessive perturbation of the PZT film 12, thereby affecting the growth of the structural layer 2 formed by low-temperature PECVD, bringing risks such as mechanical and electrical nonlinearity, and reducing the linear working range of the device.
[0067] Optionally, the longitudinal projection area of the PZT upper electrode 13 is smaller than the longitudinal projection area of the PZT thin film 12 , and the structural layer 2 is disposed on the surface of the PZT upper electrode 13 and extends to the surface of the PZT thin film 12 .
[0068] Optionally, the material of the structural layer 2 is silicon oxide and / or silicon nitride.
[0069] Optionally, the structural layer 2 is a double-layer structure in which silicon nitride and silicon oxide are stacked in sequence, such as Fig. 9 As shown, the thickness of silicon oxide is much greater than that of silicon nitride.
[0070] Optionally, the structural layer 2 is a double-layer structure in which silicon oxide and silicon nitride are stacked in sequence, such as Fig.10 As shown, the thickness of silicon nitride is much greater than the thickness of silicon oxide.
[0071] Optionally, the structural layer 2 is a three-layer structure in which silicon nitride, silicon oxide and silicon nitride are stacked in sequence. Fig.11 As shown, the thickness of silicon oxide is much greater than that of silicon nitride.
[0072] Optionally, the structural layer 2 is a three-layer structure in which silicon oxide, silicon nitride and silicon oxide are stacked in sequence, such as Fig.12As shown, the thickness of silicon nitride is much greater than the thickness of silicon oxide.
[0073] Silicon nitride and silicon oxide have a large difference in Young's modulus, and their stresses are also very different under the PECVD process. Therefore, the thickness of the three layers and the process conditions can be used to adjust the perturbation of the PZT film 12 in the structural layer 2. Among them, in the three-layer structure, the main structure of the structural layer 2 is the middle layer, and the device performance is mainly determined by the material and thickness of the middle layer. The main function of the bottom layer is to improve the adhesion of the middle layer and improve the film quality. The main function of the top layer is to enhance the tensile properties of the middle layer and improve the stability of the structural layer 2. The three-layer structure is more stable and reliable, and the yield rate is improved.
[0074] Optionally, the thickness of the structural layer 2 is 0.5-25 μm, and the thickness of the structural layer 2 is greater than that of the PZT film 12. Optionally, the structural layer 2 is deposited on the surface of the piezoelectric layer 1 by a low-temperature PECVD process.
[0075] Optional, such as Figure 6 and Figure 8 As shown, the surface of the PZT lower electrode 11 and the surface of the PZT upper electrode 13 are both provided with a metal layer 5, and the structural layer 2 and the PZT film 12 are penetrated by a groove with exposed metal layer 5. The material of the metal layer 5 can be a single metal such as aluminum, gold, or an alloy or compound such as aluminum-copper alloy.
[0076] Embodiment 2:
[0077] A preparation method proposed according to an embodiment of the present invention comprises the following steps:
[0078] See also Fig.13 , S1, prepare a substrate 3, the substrate 3 has a front side and a back side opposite to each other, and form a perturbation limiting layer 4 on the front side of the substrate 3 by a thermal oxidation process, which is used to control the position of the neutral layer and limit the perturbation of the piezoelectric layer 1. The substrate 3 is a low-perturbation silicon wafer; the perturbation limiting layer 4 is silicon oxide with a thickness of 10-500nm, and the perturbation limiting layer 4 is grown on the front side of the substrate 3 by a thermal oxidation process.
[0079] See also Fig.14 , S2, sputtering and growing a piezoelectric layer 1 on the surface of the disturbance limiting layer 4. The piezoelectric layer 1 includes a PZT lower electrode 11, a PZT film 12 and a PZT upper electrode 13, and the growth order is: sputtering and growing a layer of the PZT lower electrode 11 on the disturbance limiting layer 4; sputtering and growing a layer of the PZT film 12 on the PZT lower electrode 11; sputtering and growing a layer of the PZT upper electrode 13 on the PZT film 12.
[0080] The thickness of the PZT film 12 is 0.1-5 μm. Before the growth of the PZT film 12, the substrate 3, the interference limiting layer 4 and the PZT lower electrode 11 of the stacked structure are all in a flat state. After the growth of the PZT film 12, due to the stress, the overall deformation of the stacked structure occurs, and it bends downward.
[0081] See also Fig.15 , S3, sequentially patterning the PZT upper electrode 13, the PZT film 12 and the PZT lower electrode 11, the process is:
[0082] S31, etching the PZT upper electrode 13 by IBE to pattern the PZT upper electrode 13.
[0083] S32, wet etching the PZT film 12 to expose a portion of the PZT lower electrode 11.
[0084] S33 , etching the PZT lower electrode 11 by IBE to pattern the PZT lower electrode 11 , thereby completing the patterning of the piezoelectric layer 1 .
[0085] Optional, see Fig.19 , also includes the process:
[0086] S34, growing a metal layer 5 on the surface of the piezoelectric layer 1, wherein the metal layer 5 covers the exposed parts of the piezoelectric layer 1 and the disturbance limiting layer 4;
[0087] S35 , patterning the metal layer 5 , retaining a portion of the metal layer 5 on the surface of the PZT film 12 and the PZT upper electrode 13 .
[0088] See also Fig.16 and Fig. 20 , S4, growing a structural layer 2 on the surface of the piezoelectric layer 1. The structural layer 2 is deposited on the surface of the PZT upper electrode 13 and the PZT film 12 using a low-temperature PECVD process. After the structural layer 2 is deposited, the structural layer 2 is deformed in the direction of the PZT film 12 to obtain a disturbance that satisfies the piezoelectric stack structure, thereby improving the performance of the piezoelectric stack structure. The temperature of the low-temperature PECVD process is less than 290°C.
[0089] The thickness of the structural layer 2 is 0.5-25μm, and the material of the structural layer 2 is silicon oxide and / or silicon nitride, wherein silicon oxide is SiO2 and silicon nitride is Si3N4. Silicon nitride and silicon oxide are grown by PECVD, and the stress direction and magnitude are controlled by adjusting the low-temperature PECVD process parameters of temperature, time, power and chamber pressure to control the film stress, and the stress can be controlled more accurately.
[0090] Optionally, the structural layer 2 is a double-layer structure in which silicon nitride and silicon oxide are stacked in sequence, and the low-temperature PECVD process conditions are kept unchanged. When the thickness of silicon nitride is much greater than the thickness of silicon oxide, the thickness of the structural layer 2 is changed, and the disturbance of the piezoelectric stack is measured, as shown in Table 1:
[0091] Table 1. Calculation table of disturbance of Si3N4-SiO2 structural layer and piezoelectric stack
[0092]
[0093]
[0094] From the calculation results in Table 1, it can be seen that the change in thickness of the structural layer 2 under different thicknesses of the piezoelectric layer 1 affects the disturbance of the piezoelectric stack.
[0095] Optionally, the structural layer 2 is a double-layer structure in which silicon oxide and silicon nitride are stacked in sequence. Keeping the low-temperature PECVD process conditions unchanged, when a double-layer structure in which silicon oxide and silicon nitride are stacked in sequence is adopted, when the thickness of silicon oxide is much greater than that of silicon nitride, the thickness of the structural layer 2 is changed, and the disturbance of the piezoelectric stack is measured, as shown in Table 2:
[0096] Table 2 Calculation table of disturbance of SiO2-Si3N4 structure layer and piezoelectric stack
[0097]
[0098] From the calculation results in Table 2, it can be seen that the change in thickness of the structural layer 2 under different thicknesses of the piezoelectric layer 1 affects the disturbance of the piezoelectric stack.
[0099] Optionally, the structural layer 2 is a three-layer structure in which silicon oxide, silicon nitride and silicon oxide are stacked in sequence. Keeping the low-temperature PECVD process conditions unchanged, when a three-layer structure in which silicon oxide, silicon nitride and silicon oxide are stacked in sequence is adopted, when the thickness of silicon nitride is much greater than that of silicon oxide, the thickness of the structural layer 2 is changed, and the disturbance of the piezoelectric stack is measured, as shown in Table 3:
[0100] Table 3. Calculation table of disturbance of SiO2-Si3N4-SiO2 structure layer and piezoelectric stack
[0101]
[0102] From the calculation results in Table 3, it can be seen that the change in thickness of the structural layer 2 under different thicknesses of the piezoelectric layer 1 affects the disturbance of the piezoelectric stack.
[0103] Optionally, the structural layer 2 is a three-layer structure in which silicon nitride, silicon oxide and silicon nitride are stacked in sequence. Keeping the low-temperature PECVD process conditions unchanged, when a three-layer structure in which silicon nitride, silicon oxide and silicon nitride are stacked in sequence is adopted, the thickness of silicon oxide is much greater than the thickness of silicon nitride, and the thickness of the structural layer 2 is changed to measure the disturbance of the piezoelectric stack, as shown in Table 4:
[0104] Table 4. Calculation table of disturbance of Si3N4-SiO2-Si3N4 structure layer and piezoelectric stack
[0105]
[0106]
[0107] From the calculation results in Table 4, it can be seen that the change in thickness of the structural layer 2 under different thicknesses of the piezoelectric layer 1 has an impact on the disturbance of the piezoelectric stack.
[0108] It can be seen from Tables 1 to 4 that the thicker the piezoelectric layer 1, the greater the negative disturbance will be, and the thicker the structural layer 2, the greater the positive disturbance will be. Therefore, the disturbance of the piezoelectric stack can be adjusted by the thickness of the structural layer 2. The piezoelectric stack will form a final disturbance based on the stress superposition of the piezoelectric layer 1 and the structural layer 2, and the final disturbance is not necessarily negative. Therefore, the thickness of the piezoelectric layer 1 and the structural layer 2 needs to be reasonably set to achieve a negative disturbance in the final disturbance of the entire piezoelectric stack structure.
[0109] See also Fig.17 and Fig.21 S5, patterning the structure layer 2 to form the desired piezoelectric stack structure. The structure layer 2 is etched by ICP to expose the PZT upper electrode 13, the PZT lower electrode 11 and a portion of the disturbance limiting layer 4.
[0110] See also Fig.18 and Fig. 22 S6, patterning the substrate 3 by dry etching or wet etching to expose the back side of the disturbance limiting layer 4 and form a back cavity. The disturbance limiting layer 4, the piezoelectric layer 1 and the structural layer 2 corresponding to the projection area of the back cavity together form a diaphragm.
[0111] Optionally, when patterning the structural layer 2, the metal layer 5 is exposed, such as Fig.21 shown.
[0112] Optionally, in an embodiment of the present invention, a packaging structure in which the front or back side of the stacked structure is sealed to form an air or vacuum cavity may be adopted, thereby adjusting the air film or mechanical damping to further improve the performance of the device.
[0113] The piezoelectric stacked structure and manufacturing method proposed in the present invention utilize the characteristics that the residual stress in the growth process of the PZT film is manifested as tensile stress, so that the stacked structure has a large negative direction disturbance. First, the growth and patterning of the PZT film (piezoelectric layer) are completed, and then the structural layer is deposited on the piezoelectric layer through the PECVD process. The process parameters of the PECVD are adjusted to adjust the stress direction and size of the structural layer, so as to achieve the purpose of deformation and deflection of the structural layer toward the piezoelectric layer. The effective working range from the neutral plane to the piezoelectric layer satisfies that the disturbance direction is the direction of the structural layer toward the piezoelectric layer, that is, one side of the piezoelectric layer bulges outward (such as Figure 3 B), thereby solving the above-mentioned problems and obtaining a piezoelectric stack structure that is beneficial to improving device performance.
[0114] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A piezoelectric stack structure, comprising a substrate (3), wherein the substrate (3) has a front side and a back side opposite to each other, Features: It also includes a disturbance limiting layer (4), a piezoelectric layer (1) and a structural layer (2) which are sequentially stacked on the front side of the substrate (3); the piezoelectric layer (1) is bent and deformed in the direction of the substrate (3); the negative disturbance caused by the residual stress of the piezoelectric layer (1) is used to make the structural layer (2) bend and deform in the direction of the piezoelectric layer (1), so that the initial disturbance of the piezoelectric stack structure is in the negative direction, and the residual stress and vibration stress from the neutral surface of the piezoelectric stack structure to the effective working area of the piezoelectric layer (1) are superimposed.
2. The piezoelectric stack structure according to claim 1, It is characterized in that A back cavity is formed on the back side of the substrate.
3. The piezoelectric stack structure according to claim 2, It is characterized in that The substrate (3) is a silicon wafer substrate.
4. The piezoelectric stack structure according to claim 3, It is characterized in that The piezoelectric layer (1) comprises a PZT lower electrode (11), a PZT film (12) and a PZT upper electrode (13) which are stacked in sequence, and the disturbance direction of the PZT film (12) is a negative direction.
5. The piezoelectric stack structure according to claim 4, It is characterized in that The thickness of the PZT film (12) is 0.1-5 μm.
6. The piezoelectric stack structure according to claim 4, It is characterized in that The thickness of the structural layer (2) is greater than the thickness of the PZT thin film (12).
7. The piezoelectric stack structure according to claim 4, It is characterized in that Metal layers (5) are grown on the surfaces of the PZT lower electrode (11) and the PZT upper electrode (13) respectively, which facilitate the extraction of the electrodes.
8. The piezoelectric stack structure according to claim 4, It is characterized in that The longitudinal projection area of the PZT upper electrode (13) is smaller than the longitudinal projection area of the PZT thin film (12), and the structural layer (2) is arranged on the surface of the PZT upper electrode (13) and extends to the surface of the PZT thin film (12).
9. The piezoelectric stack structure according to claim 1, It is characterized in that The material of the disturbance limiting layer (4) is silicon oxide, and the thickness of the disturbance limiting layer (4) is 10-500 nm.
10. The piezoelectric stack structure according to claim 8, It is characterized in that The material of the structural layer (2) is silicon oxide and / or silicon nitride, and the thickness of the structural layer (2) is 0.5-25 μm.
11. The piezoelectric stack structure according to claim 10, It is characterized in that The structural layer (2) is a double-layer structure or a triple-layer structure in which silicon oxide and silicon nitride are alternately stacked.
12. A piezoelectric stack manufacturing method for forming the piezoelectric stack structure according to any one of claims 1 to 11 above, It is characterized in that Includes steps: S1, growing a disturbance limiting layer (4) on the front side of the substrate (3) by a thermal oxidation process; S2, sputtering and growing a piezoelectric layer (1) on the disturbance limiting layer (4), wherein the piezoelectric layer (1) bends and deforms toward the substrate (3) due to its own stress; S3, patterning the piezoelectric layer (1); S4, growing a structural layer (2) on the patterned piezoelectric layer (1), wherein the structural layer (2) is bent and deformed in the direction of the piezoelectric layer (1); S5, graphing the structural layer (2); S6, etching the back side of the substrate (3) to form a back cavity; The piezoelectric layer (1) is bent and deformed in the direction of the substrate (3), and the negative disturbance caused by the residual stress of the piezoelectric layer (1) is utilized, and the structural layer (2) is bent and deformed in the direction of the piezoelectric layer (1), so that the initial disturbance of the piezoelectric stack structure is in the negative direction, so that the residual stress and vibration stress from the neutral surface of the piezoelectric stack structure to the effective working area of the piezoelectric layer (1) are superimposed.
13. The method for manufacturing a piezoelectric stack according to claim 12, It is characterized in that In S2, a piezoelectric layer (1) is sputter-grown on the disturbance limiting layer (4), comprising: S21, sputtering and growing a layer of PZT lower electrode (11) on the disturbance limiting layer (4); S22, sputtering and growing a layer of PZT film (12) on the PZT lower electrode (11), wherein the PZT film (12) bends and deforms toward the PZT lower electrode (11) due to its own stress; S23, sputtering and growing a layer of PZT upper electrode (13) on the PZT film (12), wherein the PZT upper electrode (13) bends and deforms along the bending direction of the PZT film (12).
14. The method for manufacturing a piezoelectric stack according to claim 12, It is characterized in that The step S3 of patterning the piezoelectric layer (1) comprises: S31, etching the PZT upper electrode (13) by IBE to pattern the PZT upper electrode (13); S32, wet etching the PZT film (12) to expose a portion of the PZT lower electrode (11); S33, using IBE to etch the PZT lower electrode (11) to pattern the PZT lower electrode (11), thereby completing the patterning of the piezoelectric layer (1).
15. The method for manufacturing a piezoelectric stack according to claim 14, It is characterized in that Also includes: S34, growing a metal layer (5) on the surface of the piezoelectric layer (1), wherein the metal layer (5) covers the exposed areas of the piezoelectric layer (1) and the disturbance limiting layer (4); S35, patterning the metal layer (5), retaining a portion of the metal layer (5) on the surface of the PZT upper electrode (11) and the PZT upper electrode (13).
16. The method for manufacturing a piezoelectric stack according to claim 12, It is characterized in that The structural layer (2) is generated by adopting a low-temperature PECVD process, and the structural layer (2) is a double-layer structure or a triple-layer structure in which silicon oxide and silicon nitride are alternately stacked in sequence.