Preparation method and application of rare earth modified nano zinc oxide composite material

By modifying rare earth oxides on coronal nano zinc oxide microtube arrays, using atomic layer deposition, magnetron sputtering and hydrothermal reactions, the problem of insufficient photoelectric detection performance of nano zinc oxide materials is solved, and higher photoelectricity is achieved Catalytic performance and sensitivity, suitable for large-scale production.

CN118341417BActive Publication Date: 2024-11-26GUANGZHOU DETELOGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410462982.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-17
Publication Date
2024-11-26
Estimated Expiration
2044-04-17

AI Technical Summary

Technical Problem

In photoelectric detection, existing nano zinc oxide materials have problems such as wide band gap, limited light absorption to the ultraviolet light region, low utilization rate of sunlight and low quantum yield. The rare earth cerium ion modification method is cumbersome and costly. Difficult to mass production.

Method used

On the basis of the coronal nano zinc oxide microtube array, the rare earth oxide film is modified by atomic layer deposition technology, and the rare earth oxide film is prepared by magnetron sputtering method, and the coronal nano rare earth oxide structure is formed by hydrothermal reaction and electrodeposition method. Improve photoelectric catalytic performance.

Benefits of technology

It significantly improves the photoelectric catalytic performance, provides a stable and easy-to-use, repeatable rare earth modification method, suitable for large-scale production, and improves the photocatalytic performance and sensitivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118341417B_ABST
    Figure CN118341417B_ABST
Patent Text Reader

Abstract

The present application relates to the field of nano zinc oxide composite materials, and more specifically, it relates to a preparation method and application of a composite layer material of rare earth modified nano zinc oxide. A rare earth oxide film is modified by atomic layer deposition technology, a rare earth oxide film is prepared by magnetron sputtering, and then the rare earth oxide film is placed in a mixed liquid for hydrothermal reaction, plasma etching is used to obtain a crown-shaped nano rare earth oxide structure, and an electrodeposition method is used to obtain a rare earth modified crown nano oxide composite layer structure. The preparation method specifically modifies rare earth elements on the basis of a crown nano zinc oxide microtube array, and this method has better photoelectrocatalytic performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of preparation of nano zinc oxide composite materials, and more specifically, to a preparation method and application of a rare earth modified nano zinc oxide composite material. Background Art

[0002] Silicon-based semiconductor materials have a narrow bandgap and absorb a large amount of visible light. The interference of visible light needs to be eliminated during preparation, and the sensitivity is poor, which greatly limits their application. This type of semiconductor zinc oxide has been widely studied in the field of semiconductor ultraviolet detector materials because of its abundant and cheap raw materials, relatively simple preparation, and stable chemical properties. In addition, this type of semiconductor hardly absorbs visible light, has strong anti-interference ability, and is resistant to high temperatures, making it an ideal material for ultraviolet photodetectors.

[0003] Nano zinc oxide is one of the few oxide semiconductor materials that can achieve quantum size effect. It is an ideal semiconductor catalytic material and can be widely used in solar cells, liquid crystal displays, surface acoustic wave devices, pressure-sensitive devices, gas sensors, etc. However, it has the problems of wide band gap, light absorption limited to the ultraviolet light region, low utilization of sunlight and low quantum yield.

[0004] The existing technical solution is to use nano zinc oxide as a carrier to prepare rare earth cerium ion doped nano zinc oxide composite powder (Ce 4+ / ZnO) and effectively improved the photocatalytic efficiency.

[0005] Existing nano zinc oxide materials used for photoelectric detection have the problems of wide band gap, light absorption limited to the ultraviolet light region, low utilization rate of sunlight and low quantum yield. The method of modifying rare earth cerium ions is relatively cumbersome, costly and difficult to mass produce. The present invention aims to provide a method for preparing a rare earth modified nano zinc oxide composite layer, specifically modifying rare earth elements on the basis of a crown-shaped nano zinc oxide microtube array, which has better photoelectric catalytic performance. Summary of the invention

[0006] The present disclosure provides a preparation method of a rare earth modified nano zinc oxide composite layer material and its application. The preparation method specifically modifies rare earth elements on the basis of a crown-shaped nano zinc oxide microtube array, and this method has better photoelectrocatalytic performance.

[0007] In a first aspect, the present disclosure provides a composite layer material of rare earth modified nano zinc oxide, wherein a rare earth oxide film is modified by atomic layer deposition technology, a rare earth oxide film is prepared by magnetron sputtering, the rare earth oxide film is placed in a mixed liquid for hydrothermal reaction, plasma etching is used to obtain a crown-shaped nano rare earth oxide structure, and an electrodeposition method is used to obtain a modified crown-shaped nano rare earth oxide composite layer structure.

[0008] Preferably, the rare earth oxide film has a thickness of 10-15 nm, and the hydrothermal reaction time is 120-180 min.

[0009] Preferably, the rare earth oxides include cerium oxide, neodymium oxide and zinc oxide.

[0010] In a second aspect, the present disclosure provides a method for preparing a rare earth modified nano zinc oxide composite layer material, comprising the following steps:

[0011] S1: Preparation of zinc oxide thin film: A layer of zinc oxide thin film is modified on the substrate surface by atomic layer deposition technology. Specifically, diethyl zinc and water are used as precursor sources, and nitrogen is used as purge gas and carrier fluid. First, diethyl zinc precursor is introduced for 60-80ms, then nitrogen purge gas is introduced for 20s, and finally water vapor is introduced for 60-80ms to allow diethyl zinc adsorbed on the substrate surface to react with water vapor to generate zinc oxide. The process is repeated 1000 times; a layer of zinc oxide thin film is sputtered on the substrate surface by magnetron sputtering;

[0012] S2: Preparation of crown-shaped nano zinc oxide: placing a substrate modified with a zinc oxide film in a mixture of zinc sulfate and hexamethylenetetramine for hydrothermal reaction, followed by plasma etching, specifically using an Ar / O2 mixed gas as etching gas, to obtain a crown-shaped nano zinc oxide structure;

[0013] S3: Preparation of rare earth modified nano zinc oxide composite layer: The electrodeposition method is adopted, the substrate modified with crown-shaped nano zinc oxide is the working electrode, the platinum sheet is the auxiliary electrode, and the Ag / AgCl electrode is the reference electrode; the lanthanum oxide deposition solution is a lanthanum nitrate solution, the current density is 0.10-0.20ASD, and the electrodeposition time is 10-15min to obtain a crown-shaped nano zinc oxide composite layer structure modified with lanthanum oxide.

[0014] Preferably, in step S1, the temperature of the reaction of diethyl zinc and water vapor is 125-130°C.

[0015] Preferably, in step S2, the concentration of the zinc sulfate and hexamethylenetetramine mixed solution is 0.02M, the etching time is 5-10min, and the etching power is 100-120W.

[0016] Preferably, in step S3, the concentration of the lanthanum nitrate solution is 5 to 15 mM.

[0017] Preferably, the rare earth oxide particles are evenly distributed on the surface of the crown structure, and the particle size of the rare earth oxide particles is 5-10 nm.

[0018] Preferably, the electrodeposition reaction conditions of cerium oxide are: using 15-30 mM cerium nitrate as the deposition solution, the current density is 0.10 ASD, and the electrodeposition time is 20 min.

[0019] In a third aspect, the present disclosure provides an application of a composite layer material of rare earth modified nano zinc oxide, wherein the composite layer material is used as an oxide semiconductor material in a solar cell.

[0020] In summary, this application has the following beneficial effects:

[0021] 1. Due to the preparation method of modifying rare earth oxide on the crown-shaped nano zinc oxide structure of the present application, on the basis of the extremely large specific surface area provided by the crown structure, the rare earth oxide nanoparticles greatly increase the active sites and catalytic performance, greatly improving the photocatalytic performance of the overall structure;

[0022] 2. This application provides a method for repeatable and controllable rare earth modified crown nano zinc oxide composite structure, the preparation method is stable and easy, and can be used for large-scale production;

[0023] 3. The rare earth modified crown-shaped nano zinc oxide composite structure prepared in this application has excellent photocatalytic performance.

[0024] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not intended to limit the scope of protection of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] 1. Figure 1 It is a microtubule structure diagram of zinc oxide in this application;

[0026] 2. Figure 2 is a SEM image of the spiked crown-shaped nano zinc oxide structure in this application;

[0027] 3. Figure 3 This is a performance test diagram of the rare earth modified nano zinc oxide composite layer in this application. DETAILED DESCRIPTION

[0028] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.

[0029] Example

[0030] Example 1

[0031] A method for preparing a rare earth modified nano zinc oxide composite material comprises the following steps:

[0032] 1. Preparation of crown-shaped nano zinc oxide structures

[0033] (1) Preparation of zinc oxide film: A layer of zinc oxide film is modified on the substrate surface by atomic layer deposition technology. Specifically, diethyl zinc and water are used as precursor sources, and nitrogen is used as purge gas and carrier fluid. First, diethyl zinc precursor is introduced for 80 ms, then nitrogen purge gas is introduced for 20 s, and finally water vapor is introduced for 80 ms to allow diethyl zinc adsorbed on the substrate surface to react with water vapor to generate zinc oxide. The reaction temperature is 130 ° C, and the process is repeated 1000 times; a layer of zinc oxide film with a thickness of 15 nm can also be sputtered on the substrate surface by magnetron sputtering.

[0034] (2) Preparation of crown-shaped nano zinc oxide: The substrate modified with zinc oxide film was placed in a mixture of zinc sulfate and hexamethylenetetramine with a concentration of 0.02 M for hydrothermal reaction. The reaction time was 180 min. Then plasma etching was performed, specifically using Ar / O2 mixed gas as etching gas. The etching time was set to 10 min and the etching power was set to 120 W to obtain a crown-shaped nano zinc oxide structure.

[0035] The above preparation methods are existing technologies, such as atomic deposition method, hydrothermal method and plasma etching process, which all have mature theories. The crown-shaped nano zinc oxide materials prepared above have a crown-shaped morphology. The above is a complete and repeatable preparation process.

[0036] 2. Preparation of rare earth modified nano zinc oxide composite layer

[0037] The electrodeposition method was adopted, with the above-mentioned substrate modified with crown-shaped nano-zinc oxide as the working electrode, the platinum sheet as the auxiliary electrode, and the Ag / AgCl electrode as the reference electrode; the lanthanum oxide deposition solution was 15 mM lanthanum nitrate solution, the current density was 0.20 ASD, and the electrodeposition time was 15 min to obtain a crown-shaped nano-zinc oxide composite layer structure modified with lanthanum oxide.

[0038] Example 2

[0039] A method for preparing a rare earth modified nano zinc oxide composite material comprises the following steps:

[0040] 1. Preparation of crown-shaped nano zinc oxide structures

[0041] (1) Preparation of zinc oxide film: A zinc oxide film is modified on the substrate surface by atomic layer deposition technology. Specifically, diethyl zinc and water are used as precursor sources, and nitrogen is used as purge gas and carrier fluid. First, diethyl zinc precursor is introduced for 75ms, then nitrogen purge gas is introduced for 20s, and finally water vapor is introduced for 70ms to allow diethyl zinc adsorbed on the substrate surface to react with water vapor to generate zinc oxide. The reaction temperature is 128°C, and the process is repeated 1000 times. A zinc oxide film with a thickness of 12nm can also be sputtered on the substrate surface by magnetron sputtering.

[0042] (2) Preparation of crown-shaped nano zinc oxide: The substrate modified with zinc oxide film was placed in a mixture of zinc sulfate and hexamethylenetetramine with a concentration of 0.02 M for hydrothermal reaction. The reaction time was 150 min. Then plasma etching was performed, specifically using Ar / O2 mixed gas as etching gas. The etching time was set to 7 min and the etching power was set to 110 W to obtain a crown-shaped nano zinc oxide structure.

[0043] The above preparation methods are existing technologies, such as atomic deposition method, hydrothermal method and plasma etching process, which all have mature theories. The crown-shaped nano zinc oxide materials prepared above have a crown-shaped morphology. The above is a complete and repeatable preparation process.

[0044] 2. Preparation of rare earth modified nano zinc oxide composite layer

[0045] The electrodeposition method was adopted, with the above-mentioned substrate modified with crown-shaped nano-zinc oxide as the working electrode, the platinum sheet as the auxiliary electrode, and the Ag / AgCl electrode as the reference electrode; the lanthanum oxide deposition solution was 11 mM lanthanum nitrate solution, the current density was 0.15 ASD, and the electrodeposition time was 12 min to obtain a crown-shaped nano-zinc oxide composite layer structure modified with lanthanum oxide.

[0046] Example 3

[0047] A method for preparing a rare earth modified nano zinc oxide composite material comprises the following steps:

[0048] 1. Preparation of crown-shaped nano zinc oxide structures

[0049] (1) Preparation of zinc oxide film: A zinc oxide film is modified on the substrate surface by atomic layer deposition technology. Specifically, diethyl zinc and water are used as precursor sources, and nitrogen is used as purge gas and carrier fluid. First, diethyl zinc precursor is introduced for 60ms, then nitrogen purge gas is introduced for 20s, and finally water vapor is introduced for 60ms to allow diethyl zinc adsorbed on the substrate surface to react with water vapor to generate zinc oxide. The reaction temperature is 125°C, and the process is repeated 1000 times; a zinc oxide film with a thickness of 10nm can also be sputtered on the substrate surface by magnetron sputtering.

[0050] (2) Preparation of crown-shaped nano zinc oxide: The substrate modified with zinc oxide film was placed in a mixture of zinc sulfate and hexamethylenetetramine with a concentration of 0.02 M for hydrothermal reaction. The reaction time was 120 min. Then plasma etching was performed, specifically using Ar / O2 mixed gas as etching gas. The etching time was set to 5 min and the etching power was set to 100 W to obtain a crown-shaped nano zinc oxide structure.

[0051] The above preparation methods are existing technologies, such as atomic deposition method, hydrothermal method and plasma etching process, which all have mature theories. The crown-shaped nano zinc oxide materials prepared above have a crown-shaped morphology. The above is a complete and repeatable preparation process.

[0052] 2. Preparation of rare earth modified nano zinc oxide composite layer

[0053] The electrodeposition method was adopted, with the above-mentioned substrate modified with crown-shaped nano-zinc oxide as the working electrode, the platinum sheet as the auxiliary electrode, and the Ag / AgCl electrode as the reference electrode; the lanthanum oxide deposition solution was 5 mM lanthanum nitrate solution, the current density was 0.10 ASD, and the electrodeposition time was 10 min to obtain a crown-shaped nano-zinc oxide composite layer structure modified with lanthanum oxide.

[0054] Figure 1 This is a diagram of the zinc oxide microtube structure. The zinc oxide hollow microtubes are prepared by atomic deposition method. If the reaction time is too long or the power is too high, the integrity of the overall structure will be affected.

[0055] Figure 2 This is the SEM image of the spiked crown-shaped nano zinc oxide structure. After hydrothermal reaction growth and secondary growth of plasma etching, it has a specific crown-like hierarchical structure. After hydrothermal growth, a layer of zinc oxide nanowires is generated on the surface of the substrate, which is difficult to be destroyed during the etching process. The etching time or etching power can be appropriately increased to obtain a larger specific surface area.

[0056] Performance test of rare earth modified nano zinc oxide composite layer

[0057] The substrate layer modified with the rare earth modified nano zinc oxide composite layer is prepared as a photoelectric detection module, specifically using silver paste as the electrode coating.

[0058] Figure 3Figure (b) shows the IV curve of the module measured under dark conditions. The resistance is relatively large between -5 and 5V, and the nano zinc oxide forms a good ohmic contact with the silver electrode. Under light conditions, the current of the device rises to the order of 10-6A, but the linear relationship of the IV curve of the device has a certain deviation compared with the dark conditions. This is mainly due to the continuous separation of photogenerated electrons and holes inside zinc oxide under ultraviolet radiation conditions. Under the action of the built-in electric field, the recombination of electrons and holes is reduced, which effectively enhances the generation of photogenerated carriers and increases the life of carriers. Therefore, the photoelectric response is strong. Under the influence of photogenerated electrons and holes, the IV curve of the device under ultraviolet radiation is not a strict linear relationship.

[0059] Figure 3 Figure (c) shows the IT curve of the device under 1V bias, with the UV lamp switched on and off every 150s. The response current rises from 5.13×10-8A in the dark to 0.48×10-6A in the light, and the ratio of photocurrent to dark current, i.e. sensitivity, is more than 8 times. After three cycles of switching tests, the device has a stable and continuous response under UV light conditions.

[0060] Example 4

[0061] A method for preparing a rare earth modified nano zinc oxide composite material comprises the following steps:

[0062] 1. Preparation of crown-shaped nano zinc oxide structures

[0063] (2) Preparation of zinc oxide film: A zinc oxide film is modified on the substrate surface by atomic layer deposition technology. Specifically, diethyl zinc and water are used as precursor sources, and nitrogen is used as purge gas and carrier fluid. First, diethyl zinc precursor is introduced for 80 ms, then nitrogen purge gas is introduced for 20 s, and finally water vapor is introduced for 80 ms to allow diethyl zinc adsorbed on the substrate surface to react with water vapor to generate zinc oxide. The reaction temperature is 130 ° C, and the process is repeated 1000 times; magnetron sputtering can also be used to sputter a zinc oxide film on the substrate surface with a thickness of 15 nm.

[0064] (2) Preparation of crown-shaped nano zinc oxide: The substrate modified with zinc oxide film was placed in a mixture of zinc sulfate and hexamethylenetetramine with a concentration of 0.02 M for hydrothermal reaction. The reaction time was 180 min. Then plasma etching was performed, specifically using Ar / O2 mixed gas as etching gas. The etching time was set to 10 min and the etching power was set to 120 W to obtain a crown-shaped nano zinc oxide structure.

[0065] The above preparation methods are existing technologies, such as atomic deposition method, hydrothermal method and plasma etching process, which all have mature theories. The crown-shaped nano zinc oxide materials prepared above have a crown-shaped morphology. The above is a complete and repeatable preparation process.

[0066] 2. Preparation of rare earth modified nano zinc oxide composite layer

[0067] The electrodeposition method was adopted, with the substrate modified with crown-shaped nano-zinc oxide as the working electrode, the platinum sheet as the auxiliary electrode, and the Ag / AgCl electrode as the reference electrode; the neodymium oxide deposition solution was 10 mM neodymium carbonate solution, and the current density was 4 A / dm 2 The electrodeposition time was 15 min, and a crown-shaped nano-zinc oxide composite layer structure modified with lanthanum oxide was obtained.

[0068] Comparative Example

[0069] Comparative Example 1

[0070] The composite layer material of rare earth modified nano zinc oxide was prepared according to the method of Example 2, except that the rare earth modified nano zinc oxide was not modified by electrodeposition.

[0071] Comparative Example 2

[0072] The composite layer material of rare earth modified nano zinc oxide was prepared according to the method of Example 2, except that the crown-shaped nano zinc oxide was replaced by ordinary zinc oxide material.

[0073] The above is only an exemplary embodiment of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present disclosure should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.

Claims

1. An application of a rare earth modified nano zinc oxide composite material, characterized in that: The composite layer material is used as an oxide semiconductor material in a solar cell. The preparation method of the composite layer material comprises the following steps: S1: Preparation of zinc oxide thin film: A layer of zinc oxide thin film is modified on the substrate surface by atomic layer deposition technology. Specifically, diethyl zinc and water are used as precursor sources, and nitrogen is used as purge gas and carrier fluid. First, diethyl zinc precursor is introduced for 60-80ms, then nitrogen purge gas is introduced for 20s, and finally water vapor is introduced for 60-80ms to allow diethyl zinc adsorbed on the substrate surface to react with water vapor to generate zinc oxide. The process is repeated 1000 times; S2: Preparation of crown-shaped nano zinc oxide: placing a substrate modified with a zinc oxide film in a mixture of zinc sulfate and hexamethylenetetramine for hydrothermal reaction, followed by plasma etching, specifically using an Ar / O2 mixed gas as etching gas, to obtain a crown-shaped nano zinc oxide structure; S3: Preparation of rare earth modified nano zinc oxide composite layer: using the electrodeposition method, the substrate modified with the crown-shaped nano zinc oxide structure is used as the working electrode, and is placed in the electrodeposition solution, the platinum sheet is used as the auxiliary electrode, and the Ag / AgCl electrode is used as the reference electrode to obtain the rare earth modified nano zinc oxide composite structure; The electrodeposition solution is a lanthanum nitrate solution, the current density is 0.10-0.20 ASD, the electrodeposition time is 10-15 min, and a crown-shaped nano zinc oxide composite layer structure modified with lanthanum oxide is obtained; The rare earth oxide particles are evenly distributed on the surface of the crown structure, and the particle size of the rare earth oxide particles is 5-10nm.

2. The application of the composite layer material of rare earth modified nano zinc oxide according to claim 1, characterized in that: In step S3, the concentration of the lanthanum nitrate solution is 5-15 mM.