A high-strength concrete viscosity-reducing water-reducing agent and preparation method thereof
By using functional monomers and nano calcium carbonate compound in high-strength concrete and combining benzoic anhydride modified monomers, the problem of poor water reduction rate and stability of polycarboxylic acid water reducing agent in high-strength concrete is solved, and the problem of poor water reduction rate and stability of polycarboxylic acid water reducing agent in high-strength concrete is achieved. Good concrete fluidity and viscosity reduction effect improve the comprehensive performance and durability of concrete.
Patent Information
- Application Number
- CN202410476750.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-04-19
AI Technical Summary
The existing polycarboxylic acid water reducing agent has poor water reduction rate and poor stability in high-strength concrete, and the viscosity reduction effect is not obvious in the later stage, which affects the use effect of concrete.
2-acrylamide-2-methylpropanesulfonic acid and 2-hydroxyethyl methacrylate phosphate are used as functional monomers. By introducing sulfonic acid groups and phosphate groups, combined with nano calcium carbonate for compounding, the The anchoring point reduces the viscosity of the cement slurry, and introduces hydrophobic groups through benzoic anhydride modified methylallyl polyoxyethylene ether to improve the flowability and stability of the concrete.
It significantly improves the water reduction rate and viscosity reduction effect of concrete, enhances the flowability and stability of concrete, extends the durability of viscosity reduction effect, and improves the comprehensive performance and durability of concrete.
Smart Images

Figure BDA0004800743430000011 
Figure BDA0004800743430000081
Abstract
Description
Technical Field
[0001] The invention relates to the field of water reducing agents, and in particular to a high-strength concrete viscosity-reducing water reducing agent and a preparation method thereof. Background Art
[0002] High-strength concrete refers to concrete with a strength of C60 or above. It is made of cement, sand, stone raw materials, water reducer, or fly ash, F ore powder, slag, silica powder and other mixtures through conventional production processes. High-strength concrete is a new building material with high compressive strength, high deformation resistance, high density and low porosity. It is widely used in high-rise buildings and long-span bridge structures.
[0003] When high-strength concrete is used, in order to improve the strength of concrete, the water-cement ratio needs to be reduced, resulting in high viscosity, slow flow rate and poor workability of the concrete mixture. In order to reduce the viscosity of high-strength concrete, the current main methods used are to optimize particle grading and compound air-entraining agents, but the optimization of particle grading has great limitations, and compounding of air-entraining agents will lead to poor compatibility and reduced strength. Therefore, it is necessary to develop new viscosity-reducing water-reducing agents for high-strength concrete.
[0004] As a commonly used concrete admixture, water reducer can effectively reduce the water-cement ratio of concrete, improve the fluidity and workability of concrete, and reduce the viscosity of concrete. Polycarboxylate water reducer belongs to the third generation of water reducer, which has great advantages in collapse control, adjustable water reduction rate, and concrete strength. However, when the existing polycarboxylate water reducer is used in high-strength concrete, it has the defects of poor water reduction rate, poor stability, and unclear viscosity reduction effect of concrete in the later stage, which affects the use effect of the water reducer. Summary of the invention
[0005] In order to improve the water reduction rate and stability of the water reducing agent and to maintain the viscosity reducing effect on concrete for a long time, the present application provides a high-strength concrete viscosity reducing water reducing agent and a preparation method thereof.
[0006] The present application provides a high-strength concrete viscosity-reducing water-reducing agent and a preparation method thereof, which adopts the following technical solutions:
[0007] In a first aspect, the present application provides a high-strength concrete viscosity-reducing water-reducing agent, which is composed of the following raw materials in parts by weight:
[0008]
[0009] The functional monomer is selected from one or more of 2-acrylamide-2-methylpropane sulfonic acid and 2-hydroxyethyl methacrylate phosphate.
[0010] By adopting the above technical solution, maleic anhydride is used as an unsaturated acid, which is more conducive to slowing down the cement hydration process, allowing some free water to participate in the flow, thereby reducing the viscosity of the cement paste. Functional monomers introduce sulfonic acid groups, phosphoric acid groups and other groups into the polycarboxylic acid system, and provide more anchoring points through the introduction of groups, so that the cement paste has better dispersibility and fluidity, thereby higher water reduction rate and better viscosity reduction effect. Polycarboxylic acid solution is selected for compounding with nano calcium carbonate, and nano particles are used as raw materials for synthesizing polycarboxylic acid water reducers. The presence of carboxylic acid, sulfonic acid, phosphoric acid and other groups reduces the agglomeration of nano particles. Nano particles can disperse cement particles, improve the fluidity of concrete and reduce the loss during the pumping process. Nano particles can fill the voids in concrete, improve the comprehensive performance of concrete, make the viscosity reduction effect of concrete more lasting, and help improve the stability and durability of concrete.
[0011] Optionally, the polyether macromonomer is selected from one or more of isopentanol polyoxyethylene ether, methyl allyl polyoxyethylene ether, and allyl polyoxyethylene ether.
[0012] By adopting the above technical solution, polyoxyethylene ether monomers with large steric hindrance are selected to reduce the agglomeration of cement particles and improve the dispersion ability.
[0013] Optionally, the polyether macromonomer is prepared by mixing methyl allyl polyoxyethylene ether and benzoic anhydride modified methyl allyl polyoxyethylene ether in a mass ratio of (8.7-9):(1:1.3), wherein the benzoic anhydride modified methyl allyl polyoxyethylene ether is prepared by reacting benzoic anhydride and methyl allyl polyoxyethylene ether in a mass ratio of (3-6):(15-18).
[0014] By adopting the above technical scheme, methyl allyl polyoxyethylene ether is modified by benzoic anhydride, a hydrophobic benzene ring is introduced into the polyether macromonomer, and a hydrophobic group is introduced into the side chain, so that the generation of bound water can be reduced and free water can be released to the maximum extent, which is beneficial to reduce viscosity and reduce added water. At the same time, the presence of benzene ring also improves the structure of concrete, which is beneficial to improve the later strength of concrete.
[0015] Optionally, the functional monomer is a mixed monomer of 2-acrylamido-2-methylpropanesulfonic acid and 2-hydroxyethyl methacrylate phosphate in a mass ratio of (1.2-1.4):(0.6-0.8).
[0016] By adopting the above technical scheme, the water reduction rate and viscosity reduction effect of concrete are improved by compounding 2-acrylamide-2-methylpropane sulfonic acid and 2-hydroxyethyl methacrylate phosphate in a specific ratio.
[0017] Optionally, the nano-calcium carbonate is a sodium sulfide solution of nano-calcium carbonate, and the nano-calcium carbonate accounts for 15%-20% of the total weight of the sodium sulfide solution of nano-calcium carbonate.
[0018] By adopting the above technical solution, sodium sulfide alkaline solution is used to dissolve nano calcium carbonate, which is beneficial to reduce the agglomeration of nano particles and better play the reinforcing role of nano calcium carbide. At the same time, sodium sulfide alkaline solution also promotes the reduction of the viscosity of cement paste.
[0019] Optionally, the initiator is one or more of ammonium persulfate, azobisisobutyronitrile, hydrogen peroxide, sodium sulfite and L-ascorbic acid; the chain transfer agent is one or more of mercaptoethanol, thioglycolic acid and sodium hypophosphite.
[0020] Optionally, the particle size of the nano calcium carbonate is 50-80 nm.
[0021] By adopting the above technical solution, the solubility of 50-80nm nano calcium carbonate in sodium sulfide solution is good and the dispersion is more uniform.
[0022] In a second aspect, the present application provides a method for preparing a high-strength concrete viscosity-reducing water-reducing agent, comprising the following steps: adding a polyether macromonomer and a portion of water into a flask, stirring and heating until the polyether macromonomer is completely dissolved, to obtain a polyether macromonomer solution;
[0023] Dissolve maleic anhydride, part of the initiator and the chain transfer agent in part of water to obtain liquid a, and dissolve the functional monomer and part of the initiator in part of water to obtain liquid b;
[0024] Add solution a and solution b dropwise to the polyether macromonomer solution, raise the temperature to 65-75°C, stir and react for 2-3 hours, and adjust the pH of the reaction solution to neutral with a NaOH solution after cooling to obtain a polycarboxylic acid solution;
[0025] The nano calcium carbonate and the polycarboxylic acid solution are mixed to obtain a viscosity reducing water reducing agent.
[0026] By adopting the above technical scheme, the method selected in the present application is simple to operate, and the obtained water reducing agent has a high water reduction rate and a good viscosity reduction effect.
[0027] Optionally, the benzoic anhydride modified methyl allyl polyoxyethylene ether is prepared by the following steps:
[0028] Mix benzoic anhydride and methyl allyl polyoxyethylene ether, heat to 60-70°C and react for 2-2.5 hours, wash the resulting crude product with saturated sodium chloride solution and sodium carbonate solution, extract with ethyl acetate, and distill off the ethyl acetate to obtain benzoic anhydride modified methyl allyl polyoxyethylene ether.
[0029] Optionally, the sodium sulfide solution of nano calcium carbonate is prepared by the following steps:
[0030] Dissolve 3-5g of sodium sulfide in 95-97g of deionized water to obtain a sodium sulfide solution, weigh corresponding masses of nano-calcium carbonate and sodium sulfide solution, add the nano-calcium carbonate to the sodium sulfide solution, and ultrasonically disperse for 10-20 minutes to obtain a sodium sulfide solution of nano-calcium carbonate.
[0031] In summary, this application has the following beneficial effects:
[0032] The present application adopts maleic anhydride as an unsaturated acid, which is more conducive to slowing down the cement hydration process and allowing part of the free water to participate in the flow, thereby reducing the viscosity of the cement paste; sulfonic acid groups, phosphoric acid groups and other groups are introduced into the polycarboxylic acid system through functional monomers to provide more anchoring points, so that the cement paste has better dispersion ability and fluidity; polycarboxylic acid solution is selected to be compounded with nano calcium carbonate, and the presence of carboxylic acid, sulfonic acid, phosphoric acid and other groups reduces the agglomeration of nanoparticles. Nanoparticles can disperse cement particles, improve the fluidity of concrete and reduce the loss in the pumping process. Nanoparticles can fill the voids in concrete, improve the comprehensive performance of concrete, make the viscosity reduction effect of concrete more lasting, and help improve the stability and durability of concrete. DETAILED DESCRIPTION
[0033] The present application is further described in detail below in conjunction with Examples 1-9 and Comparative Examples 1-2.
[0034] Preparation Example
[0035] Preparation Example 1
[0036] Preparation of benzoic anhydride modified methyl allyl polyoxyethylene ether
[0037] Mix 3g of benzoic anhydride and 15g of methyl allyl polyoxyethylene ether, add to 60°C under anhydrous conditions to react for 2h, wash the resulting crude product three times with saturated sodium chloride solution and sodium carbonate solution, then extract with ethyl acetate, remove ethyl acetate by distillation to obtain benzoic anhydride modified methyl allyl polyoxyethylene ether.
[0038] Preparation Example 2
[0039] Preparation of benzoic anhydride modified methyl allyl polyoxyethylene ether
[0040] Mix 6 g of benzoic anhydride and 18 g of methyl allyl polyoxyethylene ether, add to 70°C under anhydrous conditions and react for 2.5 hours. Wash the resulting crude product three times with saturated sodium chloride solution and sodium carbonate solution, then extract with ethyl acetate, remove ethyl acetate by distillation to obtain benzoic anhydride modified methyl allyl polyoxyethylene ether.
[0041] Preparation Example 3
[0042] Preparation of benzoic anhydride modified methyl allyl polyoxyethylene ether
[0043] Mix 5g of benzoic anhydride and 17g of methyl allyl polyoxyethylene ether, add to 65°C under anhydrous conditions to react for 2.5h, wash the resulting crude product three times with saturated sodium chloride solution and sodium carbonate solution, then extract with ethyl acetate, remove ethyl acetate by distillation to obtain benzoic anhydride modified methyl allyl polyoxyethylene ether.
[0044] Example
[0045] Example 1
[0046] Preparation of high-strength concrete viscosity-reducing water-reducing agent
[0047] 75 g of prenol polyoxyethylene ether with a molecular weight of 2400 and 170 g of water were added into a three-necked flask, and the mixture was stirred and heated until the prenol polyoxyethylene ether was completely dissolved to obtain a prenol polyoxyethylene ether solution;
[0048] 8 g of maleic anhydride, 0.3 g of hydrogen peroxide and 0.3 g of thioglycolic acid were dissolved in 50 g of water to obtain liquid a; 4 g of 2-acrylamido-2-methylpropanesulfonic acid and 0.2 g of L-ascorbic acid were dissolved in 30 g of water to obtain liquid b;
[0049] Add solution a and solution b to the isopentanol polyoxyethylene ether solution respectively for 0.5 h, heat the reaction solution to 65° C. in a water bath, stir and react for 2 h, and after cooling, adjust the pH of the reaction solution to neutral with a 30% by mass NaOH solution to obtain a polycarboxylic acid solution;
[0050] 3 g of sodium sulfide solution was dissolved in 97 g of deionized water to obtain a sodium sulfide solution, 2 g of nano calcium carbonate with an average particle size of 50 nm was added to 11.3 g of the sodium sulfide solution, and ultrasonically dispersed for 10 min to obtain a sodium sulfide solution of nano calcium carbonate;
[0051] The sodium sulfide solution of nano calcium carbonate and the polycarboxylic acid solution are mixed to obtain a viscosity-reducing water-reducing agent.
[0052] Example 2
[0053] Preparation of high-strength concrete viscosity-reducing water-reducing agent
[0054] 90 g of methyl allyl polyoxyethylene ether with a molecular weight of 2400 and 200 g of water were added into a three-necked flask, and the mixture was stirred and heated until the methyl allyl polyoxyethylene ether was completely dissolved to obtain a methyl allyl polyoxyethylene ether solution;
[0055] Dissolve 12 g of maleic anhydride, 1 g of ammonium persulfate and 0.7 g of sodium hypophosphite in 60 g of water to obtain liquid a; dissolve 7 g of 2-hydroxyethyl methacrylate phosphate and 0.5 g of L-ascorbic acid in 40 g of water to obtain liquid b;
[0056] Add solution a and solution b to the methyl allyl polyoxyethylene ether solution respectively for 1 hour, heat the reaction solution to 75°C in a water bath, stir and react for 3 hours, and after cooling, adjust the pH of the reaction solution to neutral with a 30% NaOH solution to obtain a polycarboxylic acid solution;
[0057] Dissolve 5 g of sodium sulfide solution in 95 g of deionized water to obtain a sodium sulfide solution, add 5 g of nano calcium carbonate with an average particle size of 80 nm to 20 g of the sodium sulfide solution, and ultrasonically disperse for 20 minutes to obtain a sodium sulfide solution of nano calcium carbonate;
[0058] The sodium sulfide solution of nano calcium carbonate and the polycarboxylic acid solution are mixed to obtain a viscosity-reducing water-reducing agent.
[0059] Example 3
[0060] Preparation of high-strength concrete viscosity-reducing water-reducing agent
[0061] 80 g of allyl polyoxyethylene ether with a molecular weight of 2400 and 190 g of water were added into a three-necked flask, and the mixture was stirred and heated until the allyl polyoxyethylene ether was completely dissolved to obtain an allyl polyoxyethylene ether solution;
[0062] Dissolve 10 g of maleic anhydride, 0.7 g of hydrogen peroxide and 0.5 g of mercaptoethanol in 60 g of water to obtain liquid a; dissolve 5 g of 2-hydroxyethyl methacrylate phosphate and 0.3 g of ammonium persulfate in 30 g of water to obtain liquid b;
[0063] Add solution a and solution b to the allyl polyoxyethylene ether solution respectively for 1 hour, heat the reaction solution to 70°C in a water bath, stir and react for 2.5 hours, and after cooling, adjust the pH of the reaction solution to neutral with a 30% by mass NaOH solution to obtain a polycarboxylic acid solution;
[0064] 4 g of sodium sulfide solution was dissolved in 96 g of deionized water to obtain a sodium sulfide solution, 3 g of nano calcium carbonate with an average particle size of 60 nm was added to 17 g of the sodium sulfide solution, and ultrasonically dispersed for 15 min to obtain a sodium sulfide solution of nano calcium carbonate;
[0065] The sodium sulfide solution of nano calcium carbonate and the polycarboxylic acid solution are mixed to obtain a viscosity-reducing water-reducing agent.
[0066] Example 4
[0067] Preparation of high-strength concrete viscosity-reducing water-reducing agent
[0068] The difference between the present embodiment and the embodiment 1 is that: in the present embodiment, the polyether macromonomer is 65.3 g of methyl allyl polyoxyethylene ether and 9.7 g of benzoic anhydride modified methyl allyl polyoxyethylene ether prepared in the preparation example 1.
[0069] The preparation method of the high-strength concrete viscosity-reducing water-reducing agent is the same as that in Example 1.
[0070] Example 5
[0071] Preparation of high-strength concrete viscosity-reducing water-reducing agent
[0072] The difference between the present embodiment and the embodiment 1 is that: in the present embodiment, the polyether macromonomer is 67.5 g of methyl allyl polyoxyethylene ether and 7.5 g of benzoic anhydride modified methyl allyl polyoxyethylene ether prepared in the preparation example 2.
[0073] The preparation method of the high-strength concrete viscosity-reducing water-reducing agent is the same as that in Example 1.
[0074] Example 6
[0075] Preparation of high-strength concrete viscosity-reducing water-reducing agent
[0076] The difference between the present embodiment and the embodiment 1 is that: in the present embodiment, the polyether macromonomer is selected from 66g of methyl allyl polyoxyethylene ether and 9g of benzoic anhydride modified methyl allyl polyoxyethylene ether prepared in the preparation example 3.
[0077] The preparation method of the high-strength concrete viscosity-reducing water-reducing agent is the same as that in Example 1.
[0078] Example 7
[0079] Preparation of high-strength concrete viscosity-reducing water-reducing agent
[0080] The difference between the present embodiment and the embodiment 1 is that in the present embodiment, the functional monomers are 2.4 g of 2-acrylamido-2-methylpropanesulfonic acid and 1.6 g of 2-hydroxyethyl methacrylate phosphate.
[0081] The preparation method of the high-strength concrete viscosity-reducing water-reducing agent is the same as that in Example 1.
[0082] Example 8
[0083] Preparation of high-strength concrete viscosity-reducing water-reducing agent
[0084] The difference between the present embodiment and the embodiment 1 is that in the present embodiment, the functional monomers are 2.8 g of 2-acrylamido-2-methylpropanesulfonic acid and 1.2 g of 2-hydroxyethyl methacrylate phosphate.
[0085] The preparation method of the high-strength concrete viscosity-reducing water-reducing agent is the same as that in Example 1.
[0086] Example 9
[0087] Preparation of high-strength concrete viscosity-reducing water-reducing agent
[0088] The difference between the present embodiment and the embodiment 1 is that: in the present embodiment, the polyether macromonomer is selected from 65.3 g of methyl allyl polyoxyethylene ether and 9.7 g of benzoic anhydride modified methyl allyl polyoxyethylene ether prepared in the preparation example 1;
[0089] The functional monomers used were 2.4 g of 2-acrylamido-2-methylpropanesulfonic acid and 1.6 g of 2-hydroxyethyl methacrylate phosphate.
[0090] The preparation method of the high-strength concrete viscosity-reducing water-reducing agent is the same as that in Example 1.
[0091] Example 10
[0092] Preparation of high-strength concrete viscosity-reducing water-reducing agent
[0093] The difference between the present embodiment and the embodiment 1 is that: in the present embodiment, the polyether macromonomer is selected from 66g of methyl allyl polyoxyethylene ether and 9g of benzoic anhydride modified methyl allyl polyoxyethylene ether prepared in the preparation example 3;
[0094] The functional monomers used were 2.8 g of 2-acrylamido-2-methylpropanesulfonic acid and 1.2 g of 2-hydroxyethyl methacrylate phosphate.
[0095] The preparation method of the high-strength concrete viscosity-reducing water-reducing agent is the same as that in Example 1.
[0096] Comparative Example
[0097] Comparative Example 1
[0098] The difference between this comparative example and Example 1 is that no nano calcium carbonate is added to the raw materials of this comparative example.
[0099] The preparation method of the high-strength concrete viscosity-reducing water-reducing agent is the same as that in Example 1.
[0100] Comparative Example 2
[0101] The difference between this comparative example and Example 1 is that 8 g of acrylic acid is used in the raw materials of this comparative example instead of 8 g of maleic anhydride.
[0102] The preparation method of the high-strength concrete viscosity-reducing water-reducing agent is the same as that in Example 1.
[0103] Performance Testing
[0104] The mix ratio of the high-strength concrete to be tested is: 420kg / m 3 , first-grade fly ash 80kg / m 3 , first-grade mineral powder 80kg / m 3 , 0.2-2mm sand 600kg / m 3 5-25mm stone 1100kg / m 3 , water 150kg / m 3 The viscosity-reducing water-reducing agent prepared in Examples 1-9 and Comparative Examples 1-2 was added to the high-strength concrete to be tested at a solid content of 0.18% of cement mass.
[0105] 1. Water reduction rate of cement mortar
[0106] Refer to GB / T 8077-2012 "Test Method for Homogeneity of Concrete Admixtures" and measure the water reduction rate of cement mortar according to the method of 14. First, measure the water consumption of the fluidity of the base mortar, then measure the water consumption of the fluidity of the mortar with admixtures, and calculate the water reduction rate of the mortar. Record the measurement results in Table 1.
[0107] 2. Fluidity of cement paste
[0108] Refer to GB / T 8077-2012 "Test Method for Homogeneity of Concrete Admixtures" and measure the fluidity of cement paste according to 13. In a cement paste mixer, add a certain amount of cement, admixture and water and stir. Pour the stirred paste into a truncated cone mold, lift the truncated cone mold, and measure the maximum diameter of the cement paste flowing freely on the glass surface. Record the measurement results in Table 1.
[0109] 3. Rewinding time
[0110] Referring to GB 8076-2008 "Concrete Admixtures", the viscosity of concrete is quantified by measuring the flow time of the inverted slump cone. The specific method is: invert the slump cone, add a quick-open cover to the bottom, fill it with concrete and smooth it, fix the inverted slump cone on the stand, the bottom should not be less than 500mm from the ground, quickly slide the bottom cover open, and use a stopwatch to test the concrete flow time. Record the measurement results in Table 1.
[0111] Table 1
[0112]
[0113] According to Table 1, the high-strength concrete viscosity-reducing water-reducing agent prepared in the present application uses maleic anhydride, functional monomers, and polyether macromonomers as raw materials, and is compounded with nano-calcium carbonate. The water-reducing agent is added to high-strength concrete, which can play a good role in reducing water, reducing the viscosity of concrete, and enhancing the fluidity of cement paste.
[0114] When the polyether macromonomer is compounded with methyl allyl polyoxyethylene ether and methyl allyl polyoxyethylene ether modified by benzoic anhydride, benzene ring groups are introduced into the polyether macromonomer through benzoic anhydride modification, and hydrophobic groups are introduced into the side chains of the polycarboxylic acid system, which is beneficial to release free water, thereby facilitating the improvement of water reduction rate and the reduction of viscosity.
[0115] When the functional monomers are compounded with 2-acrylamido-2-methylpropane sulfonic acid and 2-hydroxyethyl methacrylate phosphate, sulfonic acid groups and phosphate groups are introduced into the polycarboxylic acid system. Different groups provide more anchoring points for calcium ions in cement, thereby improving the dispersion ability and fluidity of cement paste and achieving better viscosity reduction effect.
[0116] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high-strength concrete viscosity-reducing water-reducing agent, characterized in that: It is composed of the following raw materials in parts by weight: 75-90 parts of polyether macromonomer; Maleic anhydride 8-12 parts; 4-7 parts of functional monomer; Initiator 0.5-1.5 parts; Chain transfer agent 0.3-0.7 parts; 2-5 parts of nano calcium carbonate; 250-300 parts of water; The polyether macromonomer is prepared by mixing methyl allyl polyoxyethylene ether and benzoic anhydride modified methyl allyl polyoxyethylene ether in a mass ratio of (8.7-9):(1:1.3), wherein the benzoic anhydride modified methyl allyl polyoxyethylene ether is prepared by reacting benzoic anhydride and methyl allyl polyoxyethylene ether in a mass ratio of (3-6):(15-18); The functional monomer is a mixed monomer of 2-acrylamide-2-methylpropane sulfonic acid and 2-hydroxyethyl methacrylate phosphate in a mass ratio of (1.2-1.4):(0.6-0.8).
2. A high-strength concrete viscosity-reducing water-reducing agent according to claim 1, characterized in that: The nano calcium carbonate is selected from a sodium sulfide solution of nano calcium carbonate, and the nano calcium carbonate accounts for 15%-20% of the total weight of the sodium sulfide solution of nano calcium carbonate.
3. A high-strength concrete viscosity-reducing water-reducing agent according to claim 1, characterized in that: The initiator is one or more of ammonium persulfate, azobisisobutyronitrile, hydrogen peroxide, sodium sulfite and L-ascorbic acid; the chain transfer agent is one or more of mercaptoethanol, thioglycolic acid and sodium hypophosphite.
4. A high-strength concrete viscosity-reducing water-reducing agent according to claim 1, characterized in that: The particle size of the nano calcium carbonate is 50-80nm.
5. The method for preparing a high-strength concrete viscosity-reducing water-reducing agent according to any one of claims 1 to 4, characterized in that: The steps include: Add a polyether macromonomer and a portion of water into a flask, and stir and heat until the polyether macromonomer is completely dissolved to obtain a polyether macromonomer solution; Dissolve maleic anhydride, part of the initiator and the chain transfer agent in part of water to obtain liquid a, and dissolve the functional monomer and part of the initiator in part of water to obtain liquid b; Add solution a and solution b dropwise to the polyether macromonomer solution, raise the temperature to 65-75°C, stir and react for 2-3 hours, and adjust the pH of the reaction solution to neutral with a NaOH solution after cooling to obtain a polycarboxylic acid solution; The nano calcium carbonate and the polycarboxylic acid solution are mixed to obtain a viscosity reducing water reducing agent.
6. The method for preparing a high-strength concrete viscosity-reducing water-reducing agent according to claim 5, characterized in that: The benzoic anhydride modified methyl allyl polyoxyethylene ether is prepared by the following steps: Mix benzoic anhydride and methyl allyl polyoxyethylene ether, heat to 60-70°C and react for 2-2.5 hours, wash the resulting crude product with saturated sodium chloride solution and sodium carbonate solution, extract with ethyl acetate, and distill off the ethyl acetate to obtain benzoic anhydride modified methyl allyl polyoxyethylene ether.
7. The method for preparing a high-strength concrete viscosity-reducing water-reducing agent according to claim 5, characterized in that: The sodium sulfide solution of nano calcium carbonate is prepared by the following steps: Dissolve 3-5g of sodium sulfide in 95-97g of deionized water to obtain a sodium sulfide solution, weigh corresponding masses of nano-calcium carbonate and sodium sulfide solution, add the nano-calcium carbonate to the sodium sulfide solution, and ultrasonically disperse for 10-20 minutes to obtain a sodium sulfide solution of nano-calcium carbonate.