A highly wear-resistant resin-based graphite material and a preparation method thereof and a slider
By combining phenolic resin and bisphenol epoxy resin with scale graphite powder and worm graphite powder, and thermal spray trimellitic anhydride treatment, a high-wear-resistant resin-based graphite material was prepared, which solved the insufficient homogeneity and friction resistance of existing materials. The problem of this problem has achieved higher self-lubricating and friction resistance, and is suitable for mechanical equipment in harsh environments.
Patent Information
- Application Number
- CN202410469106.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-04-18
AI Technical Summary
The existing resin-based graphite materials have poor homogeneity and their strength and friction resistance cannot meet the requirements for use of mechanical equipment in strict environments.
Using scale graphite powder and worm graphite powder as aggregates, combined with phenolic resin and bisphenol epoxy resin as binders, high wear-resistant resin-based graphite materials are prepared by pre-oxidation treatment and thermal spraying of trimellitic anhydride, and a layer of scale graphite is used. The adsorption properties of worm graphite enhance the self-lubricating and friction resistance of the material.
It significantly improves the self-lubricating performance and service life of the material, enhances mechanical properties and friction resistance, can meet the requirements of mechanical equipment in harsh environments, and simplifies the preparation process.
Smart Images

Figure BDA0004798392460000051 
Figure BDA0004798392460000061 
Figure BDA0004798392460000071
Abstract
Description
Technical Field
[0001] This invention pertains to graphite composite materials, and particularly relates to a high wear-resistant resin-based graphite material, its preparation method, and a slider. Background Art
[0002] A slider is a mechanical component whose main function is to move linearly or cycloidically within a guide rail. It is responsible for bearing and reducing friction, and by controlling the direction and speed of movement, it achieves functions such as mechanical movement, support, and positioning. Because certain parts of some mechanical equipment cannot be lubricated with oil (as lubricating grease would be completely dissolved by solvents), the use of oil-free, self-lubricating materials as sliders has become increasingly important in various fields.
[0003] Currently, most common slider materials are engineering plastics such as ultra-high molecular weight polyethylene. Engineering plastics exhibit high performance in self-lubrication, but due to their low strength and hardness, narrow operating temperature range, and poor thermal conductivity, they are prone to deformation, cracking, and other damage during use. Graphite, as a layered material, possesses excellent self-lubricating and thermal conductivity, enabling it to operate in harsh environments such as high temperature and high pressure. The lubrication effect of graphite is closely related to water molecules or other small molecules in the air. After adsorbing water or other small molecules, the interlayer distance increases, weakening the interlayer force and reducing shear strength, thereby improving the self-lubricating performance of graphite. However, current resin-based graphite materials have poor homogeneity, and their strength and abrasion resistance cannot meet the requirements for use in mechanical equipment under harsh environments. Summary of the Invention
[0004] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a high wear-resistant resin-based graphite material with good homogeneity and high strength and friction resistance for use in mechanical equipment under harsh environments, as well as its preparation method and slider.
[0005] To solve the above-mentioned technical problems, the technical solution proposed by this invention is as follows:
[0006] A high-wear-resistant resin-based graphite material is mainly obtained by impregnating a matrix graphite material with resin and then thermally spraying it with trimellitic anhydride. The matrix graphite material is primarily prepared from aggregates, binders, and additives in a mass ratio of 1:(0.45-0.65):(0.02-0.08). The aggregates include flake graphite powder and worm graphite powder. The unique layered structure of flake graphite creates voids between layers, and the weak van der Waals forces between layers facilitate sliding under stress, thus exhibiting excellent self-lubricating properties. Worm graphite has excellent chemical compatibility with flake graphite, and its large specific surface area and abundant microporous structure contribute to its excellent adsorption properties. When the graphite material is subjected to friction, worm graphite can adsorb small molecules in the air to a greater extent, forming a physical adsorption film, thereby synergistically increasing the material's lubrication capacity and service life.
[0007] In the above-mentioned high wear-resistant resin-based graphite material, preferably, the flake graphite powder accounts for 60 wt.%-80 wt.% of the aggregate mass, and the worm graphite powder accounts for 20 wt.%-40 wt.% of the aggregate mass.
[0008] In the above-mentioned high wear-resistant resin-based graphite material, preferably, the binder is phenolic resin and bisphenol epoxy resin.
[0009] In the aforementioned high wear-resistant resin-based graphite material, preferably, the amount of phenolic resin added is 40 wt.%-50 wt.% of the total aggregate, and the amount of bisphenol epoxy resin added is 5 wt.%-15 wt.% of the total aggregate.
[0010] In the above-mentioned high wear-resistant resin-based graphite material, preferably, the additives are trimellitic anhydride and cellulose.
[0011] In the above-mentioned high wear-resistant resin-based graphite material, preferably, the amount of trimellitic anhydride added is 1 wt.%-5 wt.% of the aggregate mass, and the amount of cellulose is 1 wt.%-3 wt.% of the aggregate mass.
[0012] Preferably, in the above-mentioned high wear-resistant resin-based graphite material, the resin used for impregnating the matrix graphite material is phenolic resin, and the amount of phenolic resin added is 2wt.%-10wt.% of the matrix graphite material.
[0013] In the above-mentioned high wear-resistant resin-based graphite material, preferably, the amount of trimellitic anhydride used in the thermal spraying is 0.4 wt.%-5 wt.% of the matrix graphite material.
[0014] As a general inventive concept, the present invention also provides a method for preparing the above-mentioned high wear-resistant resin-based graphite material, comprising the following steps:
[0015] (1) Pre-oxidize the flake graphite powder and the worm graphite powder, and then mix them evenly to obtain composite graphite powder;
[0016] (2) The composite graphite powder and the binder solution are mixed evenly in a vacuum heating environment, and then trimellitic anhydride is added under normal pressure to continue mixing to form a coated slurry. Then, the slurry is cooled by liquid nitrogen, treated by a freeze dryer, and dispersed by a depolymerizer to obtain the resin-coated mixed graphite powder.
[0017] (3) The mixed graphite powder and cellulose are kneaded at room temperature and pressure to obtain green powder;
[0018] (4) The green powder is molded and then heated and cured after demolding to obtain a matrix graphite material;
[0019] (5) The matrix graphite material is placed in a phenolic resin solution and treated in a vacuum impregnation machine for 120-180 minutes. Then the material is transferred to a thermal spraying machine for trimellitic anhydride homogenization thermal spraying. After processing, a high wear-resistant resin-based graphite material is obtained.
[0020] In the above preparation method, preferably, in step (1), the pre-oxidation treatment refers to placing flake graphite powder and worm graphite powder into a ceramic boat, heating it to 200-300℃ at a rate of 1-2℃ / min, and holding it at that temperature for 2h-3h; the composite graphite powder is obtained by thoroughly mixing the pre-oxidized flake graphite powder and worm graphite powder in a kneading pan at 60-70℃.
[0021] In the above preparation method, preferably, in step (2), the adhesive solution refers to the solution formed by fully dispersing and uniformly dispersing phenolic resin and bisphenol epoxy resin in an anhydrous ethanol solution.
[0022] In the preferred embodiment of the above preparation method, the specific preparation process of the resin-coated mixed graphite powder in step (2) is as follows: the composite graphite powder and binder solution are transferred to a mixing equipment in a vacuum heating environment with a pressure of 0.05-0.1 MPa and a temperature of 65-70℃ for 1-1.5 h. Then the pressure is raised to normal pressure, and 1 wt.%-5 wt.% trimellitic anhydride of aggregate mass is added and mixed for 20-30 min to form a coating slurry. The coating slurry is then transferred to a metal container, 3-5 L of liquid nitrogen is poured in for rapid cooling, and then transferred to a pre-cooled freeze dryer for freezing treatment at -30 to -50℃ for 24-36 h. Then it is sent to a powder deagglomeration machine for deagglomeration and dispersion, and finally sieved.
[0023] In the above preparation method, preferably, in step (3), the specific preparation process of the green powder is as follows: the mixed graphite powder is added to a kneading pot, and 1wt.%-3wt.% of cellulose by mass of aggregate is added. The mixture is then mixed for 20-30 minutes under normal temperature and pressure to obtain the green powder.
[0024] In the above preparation method, preferably, in step (4), the compression molding pressure is 20-30 MPa, the holding time is 10-15 min, and the pressure is reduced to normal pressure within 5-10 min after the holding time is completed;
[0025] The heat curing process conditions are as follows: first, heat to 50℃ at a rate of 0.5-2℃ / min and hold for 30-60 min; then heat to 100℃ at a rate of 0.5-2℃ / min and hold for 30-60 min; then heat to 150℃ at a rate of 0.5-2℃ / min and hold for 30-60 min; then heat to 200℃ at a rate of 0.5-2℃ / min and hold for 120-240 min; finally, allow to cool naturally to room temperature.
[0026] The preferred method described above, in step (5), involves the following specific steps for preparing the high-wear-resistant resin-based graphite material:
[0027] The matrix graphite material is completely immersed in a phenolic resin ethanol solution with a mass fraction of 60wt.%-70wt.%, and the solution is placed in a vacuum impregnation machine and treated at -98kPa for 120-180min. Then, the treated matrix graphite material is transferred to a thermal spraying device, and trimellitic anhydride is homogenized and sprayed onto the surface of the matrix graphite material at a temperature of 150℃-180℃. Finally, it is dried in a drying oven at 180-220℃ for 20-30min.
[0028] As a general inventive concept, the present invention provides a slider, which is made of the above-mentioned high wear-resistant resin-based graphite material or the high wear-resistant resin-based graphite material prepared by the above-mentioned preparation method.
[0029] Compared with the prior art, the advantages of the present invention are as follows:
[0030] (1) The present invention uses flake graphite powder and worm graphite powder as aggregates. The special layered structure of flake graphite creates gaps between layers and the van der Waals forces between layers are relatively weak, making it easy for the layers to slide under force, thus exhibiting excellent self-lubricating properties. Worm graphite and flake graphite have excellent chemical compatibility, and worm graphite has a large specific surface area and rich microporous structure, which creates excellent adsorption properties. When the graphite material is subjected to friction, worm graphite can adsorb small molecules in the air to a greater extent to form a physical adsorption film, thereby synergistically increasing the lubrication capacity and service life of the material.
[0031] (2) The present invention uses pre-oxidized flake graphite powder and worm graphite powder as raw materials. Pre-oxidation can improve the specific surface area and activity of the two graphite powders, promote the homogeneous bonding between graphite powder and binder, and since both flake graphite and worm graphite have excellent toughness, the graphite products can be guaranteed to have good friction resistance. At the same time, flake graphite has better mechanical properties than worm graphite, and using flake graphite as the main material can ensure that the graphite products have a high mechanical property basis.
[0032] (3) The present invention uses trimellitic anhydride and cellulose as additives. Triellitic anhydride can improve the surface activity between graphite powders and promote the binding of resin to graphite particles. Cellulose forms a unique network structure inside graphite, promotes cross-linking between graphite particles and between resin and graphite particles, and provides some pores for resin to impregnate, thereby enhancing the mechanical properties and abrasion resistance of the material.
[0033] (4) In the preparation method of the present invention, liquid nitrogen cooling and freeze dryer treatment can reduce the sedimentation behavior of graphite powder and resin in the drying process of mixed paste, and promote the homogenization of graphite.
[0034] (5) In the preparation method of the present invention, resin solution impregnation and thermal spraying curing are used to achieve the resin penetration behavior on the surface of graphite products, and the surface homogenization and densification are achieved by thermal spraying curing, which can further enhance the mechanical properties of graphite materials.
[0035] (6) In the preparation method of the present invention, by controlling the pressure of molding, the degree of bonding between resin and graphite particles is adjusted, thereby achieving the adjustment of the friction resistance and mechanical properties of resin-based graphite material in the curing stage, which can cope with different usage environments.
[0036] (7) The process method of the present invention is simple and easy to operate. Detailed Implementation
[0037] To facilitate understanding of the present invention, the present invention will be described more fully and in detail below with reference to preferred embodiments, but the scope of protection of the present invention is not limited to the following specific embodiments.
[0038] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.
[0039] Unless otherwise specified, all reagents and raw materials used in this invention are commercially available products or products that can be prepared by known methods.
[0040] Example 1:
[0041] A resin-based graphite slider material of the present invention is mainly obtained by impregnating a matrix graphite material with resin and then thermally spraying it with trimellitic anhydride. The matrix graphite material is mainly prepared from aggregates, binders, and additives in a mass ratio of 1:0.52:0.03. The aggregates include flake graphite powder and worm graphite powder; the binders are phenolic resin and bisphenol epoxy resin; and the additives are trimellitic anhydride and cellulose. Flake graphite powder accounts for 73.5 wt.% of the aggregate mass, and worm graphite powder accounts for 26.5 wt.% of the aggregate mass. The amount of phenolic resin added was 41.2 wt.% of the total aggregate, the amount of bisphenol epoxy resin added was 10.3 wt.% of the total aggregate, the amount of trimellitic anhydride added among the additives was 1.5 wt.% of the aggregate mass, and the amount of cellulose added was 1.5 wt.% of the aggregate mass; the resin used for impregnating the matrix graphite material was phenolic resin, and the amount of phenolic resin added for impregnation was approximately 5 wt.% of the matrix graphite material; the amount of trimellitic anhydride used for thermal spraying was approximately 3 wt.% of the matrix graphite material.
[0042] The preparation method of the resin-based graphite slider material in this embodiment includes the following steps:
[0043] (1) Place 500g of flake graphite powder and 180g of worm graphite powder after 425 mesh screening into a ceramic boat, and pre-oxidize it in a tube furnace at a heating rate of 2℃ / min to 280℃ for 2h. After cooling, place it into a kneading pot and mix it at 70℃ for 1h to obtain composite graphite powder.
[0044] (2) Place 280g of phenolic resin and 70g of bisphenol epoxy resin in 1750mL of anhydrous ethanol and stir thoroughly for 2h to disperse evenly and form a resin solution. Transfer the composite graphite powder and resin solution prepared in step (1) to a mixing device in a vacuum heating environment with a pressure of 0.05MPa and a temperature of 70℃ and mix for 1.5h. Then raise the pressure of the device to atmospheric pressure, add 10g of trimellitic anhydride, and continue mixing for 30min to form a coating slurry. Then transfer the coating slurry to a metal container, slowly pour in 5L of liquid nitrogen to rapidly cool the slurry, and then transfer it to a pre-cooled freeze dryer and treat it at -30℃ for 24h. Then send it to a powder depolymerization machine for depolymerization and dispersion and screen it through an 80-mesh ultrasonic vibrating screen.
[0045] (3) Place the powder obtained in step (2) into a mixing pot, add 10g of cellulose, and mix for 30 minutes under normal temperature and pressure to obtain raw powder.
[0046] (4) Place the green powder into a molding die, slowly pressurize it to 30 MPa and hold it for 10 min, then reduce the pressure to normal pressure within 10 min and take it out to obtain the green material; place the green material into a drying oven and heat it to 50°C at a rate of 1°C / min and hold it for 30 min; then heat it to 100°C at a rate of 1°C / min and hold it for 30 min; then heat it to 150°C at a rate of 1°C / min and hold it for 30 min; then heat it to 200°C at a rate of 1°C / min and hold it for 120 min; then cool it naturally to room temperature to obtain the matrix graphite material.
[0047] (5) The matrix graphite material is completely immersed in a phenolic resin ethanol solution with a mass fraction of 65 wt.%. The solution in which the matrix graphite material is immersed is then placed in a vacuum impregnation machine and treated at -98 kPa for 120 min. It is then dried at 70°C for 60 min to remove the ethanol solvent. The weight gain is about 5 wt.%. The treated matrix graphite material is then transferred to a thermal spraying device and homogenized and sprayed onto the surface of the matrix graphite material at a temperature of 180°C. The material is then dried in a drying oven at 200°C for 30 min. The weight gain is about 3 wt.% compared to the matrix graphite material. The material is then processed to obtain a high wear-resistant resin-based graphite finished product.
[0048] In this embodiment, the product qualification rate of the high wear-resistant resin-based graphite finished material was 88.4%.
[0049] The matrix graphite material obtained in step (4) and the high wear-resistant resin-based graphite material obtained in step (5) of this embodiment were processed to different corresponding sizes for performance testing in accordance with the national standards GB / T 1431-2009 for compressive strength, GB / T24525-2009 for resistivity, GB / T39535-2020 for Shore hardness, and GB / T 40398-2021 for friction performance. The results are shown in Table 1. The standard deviation of the wear coefficient is the value calculated by taking 3 samples for each embodiment and taking 5 points for each sample.
[0050] Table 1. Properties of Graphite Matrix Materials and High Wear-Resistant Resin-Based Graphite Materials
[0051]
[0052] As can be seen from Table 1, the resin-based slider material prepared by this invention has fully met and exceeded the performance requirements of slider products and can be used in slider products. In particular, its Shore hardness exceeds that of C11 by 22.7%, and its compressive strength and coefficient of friction are also superior to PA66 (ultra-high molecular weight polyethylene), a high-performance slider material currently on the market. Moreover, compared with PA66, whose upper temperature resistance limit is less than 300℃, the finished material prepared by this invention has incomparable advantages (graphite material has an upper temperature limit of 700℃ in an oxygen-rich environment and above 3000℃ in an oxygen-free environment).
[0053] Example 2:
[0054] The process in this embodiment is the same as in embodiment 1, except that the ratio of the two types of graphite powder in the aggregate is different. Flake graphite powder accounts for 68.5 wt.% of the aggregate mass, and worm graphite powder accounts for 31.5 wt.% of the aggregate mass.
[0055] In this embodiment, the product qualification rate is 89.2%.
[0056] The matrix graphite material prepared in step (4) and the high wear-resistant resin-based graphite material prepared in step (5) were processed to the corresponding dimensions according to the national standards GB / T 1431-2009 for compressive strength, GB / T24525-2009 for resistivity, GB / T 39535-2020 for Shore hardness, and GB / T 40398-2021 for friction performance, and the results are shown in Table 2.
[0057] Table 2. Properties of Graphite Matrix Materials and High Wear-Resistant Resin-Based Graphite Materials
[0058]
[0059] As shown in Table 2, the resin-based slider material prepared by this invention has fully met the performance requirements of excellent slider products in terms of compressive strength, Shore hardness and friction properties, and can be used in slider products.
[0060] Example 3:
[0061] The process in this embodiment is the same as in embodiment 1, except for the ratio of the two types of graphite powder in the aggregate: flake graphite powder accounts for 78.5 wt.% of the aggregate mass, and worm graphite powder accounts for 21.5 wt.% of the aggregate mass.
[0062] In this embodiment, the product qualification rate is 88.3%.
[0063] The matrix graphite material prepared in step (4) and the high wear-resistant resin-based graphite material prepared in step (5) were processed to the corresponding dimensions according to the national standards GB / T 1431-2009 for compressive strength, GB / T24525-2009 for resistivity, GB / T 39535-2020 for Shore hardness, and GB / T 40398-2021 for friction performance, and the results are shown in Table 3.
[0064] Table 3. Properties of Graphite Matrix Materials and High Wear-Resistant Resin-Based Graphite Materials
[0065]
[0066] As shown in Table 3, the resin-based slider material prepared by this invention has fully met the performance requirements of excellent slider products in terms of compressive strength, Shore hardness and friction properties, and can be used in slider products.
[0067] Comparative Example 1:
[0068] The graphite material in this comparative example is processed in the same way as in Example 1. The difference lies in the types of graphite powders in the aggregate. In this comparative example, the worm graphite powder in Example 1 is replaced with an equal amount of artificial graphite powder. All other proportions and processes are the same.
[0069] The product qualification rate in this comparative example is 91.3%.
[0070] The matrix graphite material prepared in step (4) and the finished material prepared in step (5) were processed to the corresponding dimensions according to national standards and their performance was tested. The results are shown in Table 4.
[0071] Table 4. Properties of the matrix graphite material and the finished material
[0072]
[0073] Comparing Tables 1 and 4, it can be concluded that although the density and mechanical properties of the finished materials have been improved and can meet the performance requirements of C11 and PA66, the performance in terms of friction coefficient and wear amount has been significantly reduced, making it difficult to meet the requirements for use of slider materials.
[0074] Comparative Example 2:
[0075] The raw material ratios in this comparative example are the same as those in Example 1. The preparation method is different from that in Example 1, omitting the pre-oxidation step of the aggregate and the freeze-drying and dispersing process of the coating material.
[0076] The preparation method of the graphite material in this comparative example includes the following steps:
[0077] (1) After drying 500g of flake graphite powder and 180g of worm graphite powder after sieving 425 mesh, put them into a mixing pot and mix them at 70℃ for 1h to obtain composite graphite powder.
[0078] (2) Place 280g of phenolic resin and 70g of bisphenol epoxy resin in 1750mL of anhydrous ethanol and stir thoroughly for 2h to disperse evenly and form a resin solution. Transfer the composite graphite powder and resin solution prepared in step (1) into a mixing pot at 70℃ and mix for 1.5h. Then add 10g of trimellitic anhydride and continue mixing for 30min to form a coating slurry. Send the coating slurry to an 80℃ drying oven to dry for 12h, then send it to a mechanical pulverizer to break it up and screen it through an 80-mesh vibrating screen.
[0079] (3) Place the powder obtained in step (2) into a mixing pot, add 10g of cellulose, and mix for 30 minutes under normal temperature and pressure to obtain raw powder.
[0080] (4) Place the green powder into a molding die, slowly pressurize it to 30 MPa and hold it for 10 min, then reduce the pressure to normal pressure within 10 min and take it out to obtain the green material; place the green material into a drying oven and heat it to 50°C at a rate of 1°C / min and hold it for 30 min; then heat it to 100°C at a rate of 1°C / min and hold it for 30 min; then heat it to 150°C at a rate of 1°C / min and hold it for 30 min; then heat it to 200°C at a rate of 1°C / min and hold it for 120 min; then cool it naturally to room temperature to obtain the matrix graphite material.
[0081] (5) The matrix graphite material is completely immersed in a phenolic resin ethanol solution with a mass fraction of 65 wt.%. The solution in which the matrix graphite material is immersed is then placed in a vacuum impregnation machine and treated at -98 kPa for 120 min. It is then dried at 70°C for 60 min to remove the ethanol solvent. The weight gain is approximately 5 wt.%. The treated matrix graphite material is then transferred to a thermal spraying device. Trimeric triacid anhydride is homogenized and sprayed onto the surface of the matrix graphite material at a temperature of 180°C. The material is then dried in a drying oven at 200°C for 30 min. The weight gain is approximately 3 wt.%. After processing, the finished material is obtained.
[0082] The product qualification rate in this comparative example is 80.2%.
[0083] The matrix graphite material prepared in step (4) and the finished material prepared in step (5) were processed to the corresponding dimensions according to national standards and their performance was tested. The results are shown in Table 5.
[0084] Table 5 Properties of Matrix Graphite Material and Finished Graphite Material
[0085]
[0086]
[0087] Comparing Tables 1 and 5, it is evident that the material properties prepared using conventional methods differ significantly from those prepared using the method employed in this invention. The sedimentation of the paste during wet mixing and solvent drying leads to unevenness in the dried green powder and agglomeration of the binder, resulting in inconsistent performance across various tests (as can be seen from the abrasion standard deviation, which is larger than that of the previous example). Furthermore, the agglomeration of the asphalt not only results in lower mechanical properties but also poorer abrasion resistance. Although the finished material meets the C11 and PA66 specifications, the sedimentation phenomenon during the preparation process is difficult to control.
Claims
1. A method for preparing a highly wear-resistant resin-based graphite material, characterized in that: The highly wear-resistant resin-based graphite material is mainly obtained by first impregnating a matrix graphite material with resin and then thermally spraying trimellitic anhydride, wherein the matrix graphite material is mainly prepared from aggregate, a binder and an additive in a mass ratio of 1: (0.45-0.65): (0.02-0.08), the aggregate includes flake graphite powder and worm graphite powder, the additive is trimellitic anhydride and cellulose, and the preparation method comprises the following steps: (1) Pre-oxidizing flake graphite powder and vermicular graphite powder, and then mixing them evenly to obtain composite graphite powder; (2) mixing the composite graphite powder and the binder solution in a vacuum heating environment, then adding trimellitic anhydride and continuing to mix under normal pressure to form a coating slurry, and then cooling with liquid nitrogen, treating with a freeze dryer, and breaking up with a depolymerizer to obtain a mixed graphite powder coated with a resin; (3) kneading the mixed graphite powder and cellulose at room temperature and pressure to obtain a green powder; (4) molding the green powder, and heating and curing the green powder after demolding to obtain a matrix graphite material; (5) Immersing the base graphite material in a phenolic resin solution, treating it in a vacuum infiltration machine for 120-180 minutes, and then transferring it to a thermal spraying machine for homogenization thermal spraying of trimellitic anhydride to obtain a highly wear-resistant resin-based graphite material.
2. The preparation method according to claim 1, characterized in that In step (1), the pre-oxidation treatment refers to placing the flake graphite powder and the worm graphite powder in a porcelain boat, heating the boat to 200-300°C at a rate of 1-2°C / min, and keeping the temperature for 2-3h; The composite graphite powder is obtained by uniformly mixing the pre-oxidized flake graphite powder and the worm graphite powder in a kneading pot at 60-70°C.
3. The preparation method according to claim 1, characterized in that: In step (2), the binder solution is formed by placing phenolic resin and bisphenol epoxy resin in an anhydrous ethanol solution and fully dispersing them evenly.
4. The preparation method according to claim 1, characterized in that: In step (2), the specific preparation process of the mixed graphite powder coated with the resin is as follows: the composite graphite powder and the binder solution are transferred to a mixing device in a vacuum heating environment with an air pressure of 0.05-0.1 MPa and a temperature of 65-70°C for mixing for 1-1.5 hours, then the air pressure is raised to normal pressure, trimellitic anhydride is added and mixing is continued for 20-30 minutes to form a coating slurry; then the coating slurry is transferred to a metal container, poured into liquid nitrogen for rapid cooling, and then transferred to a pre-cooled freeze dryer, frozen at -30 to -50°C for 24 hours to 36 hours, and finally sent to a powder depolymerizer for depolymerization and sieving.
5. The preparation method according to claim 1, characterized in that: In step (3), the specific preparation process of the green powder is: adding the mixed graphite powder into a kneading pot, adding 1 wt.%-3 wt.% of cellulose based on the mass of the aggregate, and mixing for 20-30 minutes at normal temperature and pressure to obtain the green powder.
6. The preparation method according to claim 1, characterized in that: In step (4), the pressure of the compression molding is 20-30 MPa, the holding time is 10-15 min, and after the holding time is completed, the pressure is reduced to normal pressure within 5-10 min; The process conditions for heating and curing are: first increase the temperature to 50°C at a rate of 0.5-2°C / min and keep it warm for 30-60min, then increase the temperature to 100°C at a rate of 0.5-2°C / min and keep it warm for 30-60min, then increase the temperature to 150°C at a rate of 0.5-2°C / min and keep it warm for 30-60min, then increase the temperature to 200°C at a rate of 0.5-2°C / min and keep it warm for 120-240min, and finally cool naturally to room temperature.
7. The preparation method according to claim 1, characterized in that: In step (5), the specific process of preparing the highly wear-resistant resin-based graphite material is as follows: The matrix graphite material is completely immersed in a phenolic resin ethanol solution with a mass fraction of 60 wt.%-70 wt.%, and the solution in which the matrix graphite material is immersed is placed in a vacuum infiltration machine and treated at -98 KPa for 120-180 minutes. The treated matrix graphite material is then transferred to a thermal spraying device, and trimellitic anhydride is homogenized and sprayed on the surface of the matrix graphite material at a temperature of 150°C-180°C, and then dried in a drying oven for 20-30 minutes.
8. The preparation method according to claim 1, characterized in that The flake graphite powder accounts for 60 wt.%-80 wt.% of the mass of the aggregate, and the worm graphite powder accounts for 20 wt.%-40 wt.% of the mass of the aggregate.
9. The preparation method according to claim 3, characterized in that: The amount of the phenolic resin added is 40 wt.%-50 wt.% of the total amount of aggregate, and the amount of the bisphenol epoxy resin added is 5 wt.%-15 wt.% of the total amount of aggregate.
10. The preparation method according to claim 1, characterized in that: The amount of trimellitic anhydride added in the additive is 1 wt.%-5 wt.% of the mass of the aggregate, and the amount of cellulose added is 1 wt.%-3 wt.% of the mass of the aggregate.
11. The preparation method according to claim 1, characterized in that: The impregnation amount of the phenolic resin is 2wt.%-10wt.% of the base graphite material.
12. The preparation method according to claim 1, characterized in that: The thermal spraying amount of trimellitic anhydride is 0.4 wt.%-5 wt.% of the base graphite material.
13. A slider, characterized in that: The slider is made of a highly wear-resistant resin-based graphite material prepared by the preparation method according to any one of claims 1 to 12.