A kind of high wear-resistant concrete specially used for steps and preparation method thereof

By using polyvinyl acetate emulsion, nano-concave and concave rod soil and sisal fiber in concrete, polymer film and reinforced structure are formed, which solves the problem of degradation in the sun and rain environment, and significantly improves wear resistance and compressive resistance, extending service life.

CN118344098BActive Publication Date: 2024-11-19广州市兴耀混凝土有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410536545.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-30
Publication Date
2024-11-19
Estimated Expiration
2044-04-30

AI Technical Summary

Technical Problem

The performance of existing concrete steps in sun and rainy environments will decline, resulting in damage and functional impact, and their wear resistance and compressive resistance need to be improved.

Method used

Using highly wear-resistant concrete formulas, including silicate cement, coarse aggregate, fine aggregate, mineral blends, polyvinyl acetate emulsion, nano-concave stick soil and sisal fibers, polymer films are formed through polyvinyl acetate emulsion. Nanoconcave and convex rod soil serves as a support point, and sisal fibers interspersize enhance the structure to improve fluidity and compressive resistance.

Benefits of technology

It significantly improves the wear resistance and compressive resistance of concrete, extends the performance protection aging, enhances the cohesion and stability of the structure, can effectively resist the influence of sun and rain, reduces instantaneous damage to external forces, and extends the service life of the steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004819769600000061
    Figure BDA0004819769600000061
  • Figure BDA0004819769600000081
    Figure BDA0004819769600000081
  • Figure BDA0004819769600000091
    Figure BDA0004819769600000091
Patent Text Reader

Abstract

The present application relates to the field of concrete, and more specifically, it relates to a high wear-resistant concrete dedicated to steps and a preparation method thereof. A high wear-resistant concrete dedicated to steps includes the following raw materials: 250-260 parts of Portland cement, 1100-1200 parts of coarse aggregate, 750-800 parts of fine aggregate, 40-80 parts of mineral admixtures, 1-4 parts of water reducers, 145-155 parts of water, 1-5 parts of nano-attapulgite, 5-10 parts of polyvinyl acetate emulsion, and 7-15 parts of sisal fibers; its preparation method is: mixing Portland cement, water, and mineral admixtures; mixing nano-attapulgite and polyvinyl acetate emulsion to obtain a premix; mixing the premix, sisal fibers, and materials; continuing to add fine aggregate, coarse aggregate, and water reducer to mix to obtain high wear-resistant concrete. The concrete of the present application has high wear resistance, high strength, and can withstand sun and rain, and is suitable for preparing steps.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of concrete, and more specifically, to a high wear-resistant concrete specially used for steps and a preparation method thereof. Background Art

[0002] Stairs generally refer to buildings made of bricks, stones, concrete, etc., which are used for people to go up and down. They are mostly in front of the gate or on the ramp. Stairs are also one of the important elements in architectural design, which can set off the image of the building and enrich the spatial level of the building. In modern buildings, stairs are still widely used. They not only have practical functions, but also play the role of beautifying the environment and guiding the flow of people.

[0003] The most common and widely used material for making steps is concrete, which has the advantages of low price, good performance and good molding effect. However, some steps are located outdoors and need to withstand the sun and rain for a long time. Under the influence of these factors, the performance of concrete will be greatly reduced, and it will be damaged and destroyed, which will affect the function of the steps. Therefore, there is still room for improvement. Summary of the invention

[0004] In order to improve the strength of concrete and reduce the impact of sun and rain on the performance of concrete, the present application provides a high wear-resistant concrete specially used for steps and a preparation method thereof.

[0005] In the first aspect, the present application provides a high-wear-resistant concrete specially used for steps, adopting the following technical scheme: a high-wear-resistant concrete specially used for steps, comprising at least the following raw materials, in parts by mass: 250-260 parts of Portland cement, 1100-1200 parts of coarse aggregate, 750-800 parts of fine aggregate, 40-80 parts of mineral admixture, 1-4 parts of water reducer, 145-155 parts of water, 1-5 parts of nano-attapulgite, 5-10 parts of polyvinyl acetate emulsion, and 7-15 parts of sisal fiber.

[0006] By adopting the above technical solution, polyvinyl acetate emulsion is dispersed into emulsion with water in concrete. As hydration proceeds, it dehydrates to form a viscous polymer film, which is evenly distributed inside and on the surface of the concrete. It can effectively block the influence of external water on the performance of concrete, and the polymer film can also improve the cohesion of the internal structure of the concrete.

[0007] Nano-attapulgite is wrapped in polyvinyl acetate emulsion, and nano-attapulgite exists as a supporting point in the polyvinyl acetate emulsion, making the polyvinyl acetate emulsion more integrated, further improving the strength of the formed polymer film, and extending its protective effect. In addition, the polyvinyl acetate emulsion containing nano-attapulgite plays the role of a "ball bearing" in concrete, which can effectively improve the fluidity of concrete and facilitate construction.

[0008] With the cooperation of nano-attapulgite, polyvinyl acetate emulsion and sisal fiber, sisal fiber interpenetrates and supports polyvinyl acetate emulsion containing nano-attapulgite, further improving the support force of polymer film, and making it long-lasting and stable, and well coping with environments such as sun and rain. In addition, nano-attapulgite, polyvinyl acetate emulsion and sisal fiber closely connect the entire concrete system. When the steps bear weight, they can quickly spread in the system to avoid excessive destructive force of external force on a certain part of the steps, thus making the steps more wear-resistant and pressure-resistant.

[0009] Preferably, the mass fraction of the nano-attapulgite is 3-5 parts, the mass fraction of the polyvinyl acetate emulsion is 7-9 parts, and the mass fraction of the sisal fiber is 10-14 parts.

[0010] By adopting the above technical solution, the dosage matching relationship between the three is further limited, so that the three are fully matched, which can have a better dispersion effect in the concrete system, making the polymer film more stable and having better performance.

[0011] Preferably, the nano-attapulgite is modified by the following method:

[0012] Step a: heat treating the nano-attapulgite at 200-300° C.

[0013] Step b: Mix the heat-treated nano-attapulgite with dodecyltrimethylammonium chloride and water at 60-70° C., wash and dry to obtain modified nano-attapulgite.

[0014] Nano-attapulgite is easy to agglomerate, which affects the coordination effect with polyvinyl acetate emulsion and sisal fiber. By adopting the above technical scheme, the nano-attapulgite is specially modified, and the obtained modified nano-attapulgite has a loose and porous structure, and the surface also has organic cations with long carbon chains, which are not easy to agglomerate in the system and are evenly dispersed. In addition, the special modification also enhances the mutual adsorption between the modified nano-attapulgite and the polyvinyl acetate emulsion, so that the modified nano-attapulgite is more firmly distributed in the polyvinyl acetate emulsion and is not easy to detach, so as to enhance the performance of the polymer film.

[0015] Preferably, in step a, the heat treatment is carried out at 200-300° C. for 30-60 min.

[0016] If the heat treatment temperature is too high, the structure of the nano-attapulgite will be excessively destroyed and subsequent modification will be impossible; if the heat treatment temperature is too low, the water of the nano-attapulgite cannot be removed and a specific structure cannot be formed.

[0017] By adopting the above technical solution, the heat treatment temperature of step a is further limited, so that the nano-attapulgite can remove part of the water, increase the number of pores, facilitate the modification of the subsequent step b, and generate a specific modified nano-attapulgite structure more quickly.

[0018] Preferably, in step b, the mass ratio of nano-attapulgite to dodecyltrimethylammonium chloride and water is 1:(0.01-0.05):(12-18).

[0019] By adopting the above technical scheme, the mass ratio of nano-attapulgite to dodecyltrimethylammonium chloride and water in step b is further limited, so that an electrical neutralization effect is produced between the negatively charged nano-attapulgite and the positively charged dodecyltrimethylammonium chloride, and ion exchange occurs quickly, thereby forming a modified nano-attapulgite with a specific structure.

[0020] Preferably, in step b, mixing is performed at 60-70° C. for 30-60 min.

[0021] By adopting the above technical solution, the mixing temperature of step b is further limited, so that the reaction can proceed more quickly and smoothly.

[0022] Preferably, the nano-attapulgite is 50-150 nm.

[0023] In a second aspect, the present application provides a method for preparing highly wear-resistant concrete specifically for steps, using the following technical solution:

[0024] A method for preparing highly wear-resistant concrete specially used for steps comprises the following steps:

[0025] Step 1: Mix silicate cement, water and mineral admixtures until uniform;

[0026] Step 2: Mix the nano-attapulgite and the polyvinyl acetate emulsion until uniform to obtain a premix;

[0027] Step 3: Add the premix and sisal fiber to the material in step 1 and mix until uniform;

[0028] Step 4: Continue to add fine aggregate, coarse aggregate and water reducer and mix until uniform to obtain highly wear-resistant concrete.

[0029] By adopting the above technical solution, various raw materials are mixed in the above order, so that the various raw materials have a more sufficient coordination effect, thereby ensuring that the concrete has high compression and wear resistance, and can withstand sun and rain.

[0030] In summary, this application has the following beneficial effects:

[0031] 1. Since the present application adopts polyvinyl acetate emulsion, a polymer film can be formed in the concrete system, which connects the internal structure more closely and protects the concrete surface, thereby resisting the influence of sun and rain and improving the strength.

[0032] 2. In this application, nano-attapulgite and polyvinyl acetate emulsion are preferably used, which play the role of "ball bearings" in concrete, can effectively improve the fluidity of concrete and facilitate construction.

[0033] 3. With the cooperation of nano-attapulgite, polyvinyl acetate emulsion and sisal fiber, the sisal fiber penetrates and supports the polyvinyl acetate emulsion containing nano-attapulgite, further improving the supporting force of the polymer film in a long-term and stable manner, and can also quickly and evenly diffuse the external force, making the concrete more wear-resistant and pressure-resistant. DETAILED DESCRIPTION

[0034] The present application is further described in detail below with reference to the embodiments.

[0035] The raw materials used in the following examples and comparative examples are all commercially available products.

[0036] Example

[0037] Example 1

[0038] A highly wear-resistant concrete specially used for steps comprises silicate cement, coarse aggregate, fine aggregate, mineral admixture, water reducing agent, water, nano-attapulgite, polyvinyl acetate emulsion and sisal fiber.

[0039] Among them, the silicate cement is P.042.5, which is commercially available.

[0040] The coarse aggregate may be crushed gravel, crushed stone, or pebbles, with a particle size of 5-25 mm. In this embodiment, crushed gravel with a particle size of 5-25 mm is selected.

[0041] The fine aggregate can be river sand, lake sand, or machine-made sand, with a particle size of 1-3 mm. In this embodiment, river sand with a particle size of 1-3 mm is selected.

[0042] The mineral admixture may be fly ash, slag, or steel slag; in this embodiment, fly ash is selected.

[0043] The water reducer may be a lignin sulfonate water reducer, a naphthalene-based high-efficiency water reducer, or a polycarboxylic acid-based high-performance water reducer; in this embodiment, a naphthalene-based high-efficiency water reducer is selected.

[0044] Nano-attapulgite is commercially available, and the particle size specification is 100 nm.

[0045] Polyvinyl acetate emulsion is commercially available, and in this embodiment, it was purchased from Shandong Poly Chemical Co., Ltd.

[0046] Sisal fiber is commercially available.

[0047] The specific amount of each raw material is shown in Table 1.

[0048] The present application also provides a method for preparing highly wear-resistant concrete specifically for steps, comprising the following steps:

[0049] Step 1: Mix silicate cement, water and mineral admixtures until uniform.

[0050] Step 2: Mix the nano-attapulgite with the polyvinyl acetate emulsion, and stir at 500 r / min until uniform to obtain a premix.

[0051] Step 3: Add the premix and sisal fiber to the material in step 1 and mix until uniform.

[0052] Step 4: Continue to add fine aggregate, coarse aggregate and water reducer and mix until uniform to obtain highly wear-resistant concrete.

[0053] Example 2

[0054] A highly wear-resistant concrete specially used for steps, which is different from Example 1 in that the specific amounts of various raw materials are different, see Table 1 for details.

[0055] The particle size specification of nano-attapulgite is 50nm.

[0056] Example 3

[0057] A highly wear-resistant concrete specially used for steps, which is different from Example 1 in that the specific amounts of various raw materials are different, see Table 1 for details.

[0058] The particle size specification of nano-attapulgite is 150nm.

[0059] Example 4

[0060] A highly wear-resistant concrete specially used for steps, which is different from Example 1 in that:

[0061] Nano-attapulgite is also modified by the following methods:

[0062] Step a: Place the nano-attapulgite in a muffle furnace and calcine at 250° C. for 40 minutes, then take it out and cool it to room temperature.

[0063] Step b: weigh the raw materials according to the mass ratio of nano-attapulgite, dodecyltrimethylammonium chloride and water of 1:0.03:15, that is, 3.5 kg of nano-attapulgite, 0.105 kg of dodecyltrimethylammonium chloride and 52.5 kg of water (used in this step).

[0064] Then, the nano-attapulgite prepared in step a, dodecyltrimethylammonium chloride and water were put into a reaction kettle and mixed at 65° C. for 1.5 h.

[0065] After taking out, the solid and liquid were separated, the solid part was washed with ethanol, and dried in hot air at 60° C. to constant weight to obtain modified nano-attapulgite.

[0066] The present application also provides a method for preparing highly wear-resistant concrete specifically for steps, comprising the following steps:

[0067] Step 1: Mix silicate cement, water and mineral admixtures until uniform.

[0068] Step 2: Mix the modified nano-attapulgite and polyvinyl acetate emulsion, and stir at 500 r / min until uniform to obtain a premix.

[0069] Step 3: Add the premix and sisal fiber to the material in step 1 and mix until uniform.

[0070] Step 4: Continue to add fine aggregate, coarse aggregate and water reducer and mix until uniform to obtain highly wear-resistant concrete.

[0071] Example 5

[0072] A highly wear-resistant concrete specially used for steps, which is different from Example 4 in that:

[0073] The specific amount of each raw material is different, see Table 1 for details.

[0074] Nano-attapulgite is also modified by the following methods:

[0075] Step a: Place the nano-attapulgite in a muffle furnace and calcine at 200° C. for 60 minutes, then take it out and cool it to room temperature.

[0076] Step b: weigh the raw materials according to the mass ratio of nano-attapulgite, dodecyltrimethylammonium chloride and water of 1:0.01:12, that is, 3 kg of nano-attapulgite, 0.03 kg of dodecyltrimethylammonium chloride and 36 kg of water (used in this step).

[0077] Then, the nano-attapulgite prepared in step a, dodecyltrimethylammonium chloride and water were put into a reaction kettle and mixed at 60° C. for 2 h.

[0078] After taking out, the solid and liquid were separated, the solid part was washed with ethanol, and dried in hot air at 60° C. to constant weight to obtain modified nano-attapulgite.

[0079] Example 6

[0080] A highly wear-resistant concrete specially used for steps, which is different from Example 4 in that:

[0081] The specific amount of each raw material is different, see Table 1 for details.

[0082] Nano-attapulgite is also modified by the following methods:

[0083] Step a: Place the nano-attapulgite in a muffle furnace and calcine at 300° C. for 30 minutes, then take it out and cool it to room temperature.

[0084] Step b: weigh the raw materials according to the mass ratio of nano-attapulgite, dodecyltrimethylammonium chloride and water of 1:0.05:18, that is, 5 kg of nano-attapulgite, 0.25 kg of dodecyltrimethylammonium chloride and 90 kg of water (used in this step).

[0085] Then, the nano-attapulgite prepared in step a, dodecyltrimethylammonium chloride and water were put into a reaction kettle and mixed at 70° C. for 1 hour.

[0086] After taking out, the solid and liquid were separated, the solid part was washed with ethanol, and dried in hot air at 60° C. to constant weight to obtain modified nano-attapulgite.

[0087] Table 1

[0088]

[0089] Example 7

[0090] A highly wear-resistant concrete specially used for steps, which is different from Example 4 in that the mass ratio of nano-attapulgite to dodecyltrimethylammonium chloride and water is 1:0.1:15, that is, the nano-attapulgite is 3.5 kg, the dodecyltrimethylammonium chloride is 0.35 kg, and the water (used in this step) is 52.5 kg.

[0091] Example 8

[0092] A highly wear-resistant concrete specially used for steps, which is different from Example 4 in that step a is omitted.

[0093] Example 9

[0094] A highly wear-resistant concrete specially used for steps, which is different from Example 4 in that step b is omitted.

[0095] Example 10

[0096] A highly wear-resistant concrete specially used for steps, which is different from Example 4 in that the nano-attapulgite is further modified by the following method:

[0097] Step a: weigh the raw materials according to the mass ratio of nano-attapulgite, dodecyltrimethylammonium chloride and water of 1:0.03:15, that is, 3.5 kg of nano-attapulgite, 0.105 kg of dodecyltrimethylammonium chloride and 52.5 kg of water (used in this step).

[0098] Then, the nano-attapulgite, dodecyltrimethylammonium chloride and water were put into a reaction kettle and mixed at 65° C. for 1.5 h.

[0099] After taking out, the solid and liquid were separated, the solid part was washed with ethanol, and dried in hot air at 60°C to constant weight.

[0100] Step b: Place the constant-weight nano-attapulgite in a muffle furnace and calcine at 250° C. for 40 minutes, take it out and cool it to room temperature to obtain modified nano-attapulgite.

[0101] Comparative Example

[0102] Comparative Example 1

[0103] A highly wear-resistant concrete specially used for steps, which is different from Example 1 in that the nano-attapulgite is replaced by montmorillonite.

[0104] Comparative Example 2

[0105] A highly wear-resistant concrete specially used for steps, which is different from Example 1 in that polyvinyl acetate emulsion is replaced by styrene acrylic emulsion.

[0106] Comparative Example 3

[0107] A highly wear-resistant concrete specially used for steps, which is different from Example 1 in that sisal fiber is replaced by bamboo fiber.

[0108] Comparative Example 4

[0109] A highly wear-resistant concrete specially used for steps, which is different from Example 1 in that the amount of nano-attapulgite is 8 kg, the amount of polyvinyl acetate emulsion is 13 kg, and the amount of sisal fiber is 3.5 kg.

[0110] Comparative Example 5

[0111] A highly wear-resistant concrete specially used for steps, which is different from Example 4 in that the nano-attapulgite is replaced by montmorillonite.

[0112] Comparative Example 6

[0113] A highly wear-resistant concrete specially used for steps, which is different from Example 4 in that the amount of nano-attapulgite is 8 kg, the amount of polyvinyl acetate emulsion is 13 kg, and the amount of sisal fiber is 3.5 kg.

[0114] Performance testing

[0115] 1. Compressive strength: Referring to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the concrete of Examples 1-10 and Comparative Examples 1-6 were tested for 28d compressive strength, and the results are recorded in Table 2.

[0116] 2. Abrasion resistance: The concrete of Examples 1-10 and Comparative Examples 1-6 were tested with reference to JTG 3420-2020 "Test Procedures for Cement and Cement Concrete for Highway Engineering", and the wear per unit area was recorded in Table 2.

[0117] 3. Simulation test: The concrete of Examples 1-10 and Comparative Examples 1-6 were made into test pieces and cured, and then the surfaces of the cured test pieces were continuously irradiated with a 50W ultraviolet lamp for 28 days. During the irradiation period, the test pieces were sprayed with 60°C clean water for 4 hours every day.

[0118] Then repeat Test 1 and Test 2, and record the results in Table 2.

[0119] 4. Fluidity: Test the slump according to GB / T 50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures" and record the results in Table 2.

[0120] Table 2

[0121]

[0122]

[0123] According to the comparison of the test data of Examples 1-3 and Comparative Examples 1-4 in Table 2, it can be seen that the concrete of Examples 1-3 has higher compressive strength and better wear resistance than that of Comparative Examples 1-4; in the test of simulating sun exposure and rain, it can also be seen from the data comparison that the concrete of Examples 1-3 has less impact. It shows that the combination of nano-attapulgite, polyvinyl acetate emulsion and sisal fiber gives the concrete good strength and wear resistance. The destruction mode of changing any one of the raw materials to other raw materials or changing the special dosage matching relationship between the three makes it impossible to reproduce this excellent effect.

[0124] According to the comparison of the test data of Example 1 and Examples 4-6 in Table 2, it can be seen that the strength and wear resistance of Examples 4-6 are more significantly improved than those of Example 1, and the concrete of Examples 4-6 has better resistance to external factors such as sun and rain than Examples 1-3.

[0125] According to the comparison of the test data of Example 4 and Comparative Examples 5-6 in Table 2, it can be seen that the concrete performance of Comparative Examples 5-6 is significantly lower than that of Example 4, indicating that the modification of nano-attapulgite can also have a good coordination effect with polyvinyl acetate emulsion and sisal fiber, and can further exert its coordination effect.

[0126] In Example 7-10, the modification conditions of nano-attapulgite are changed on the basis of Example 4. According to the comparison of the test data of Example 4 and Example 7-10 in Table 2, the concrete performance of Example 7-10 is reduced. This is because the modification conditions of nano-attapulgite are changed, which affects the structure of the modified nano-attapulgite, thereby affecting the coordination with polyvinyl acetate emulsion and sisal fiber, resulting in a reduction in performance.

[0127] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A highly wear-resistant concrete specially used for steps, characterized in that: According to the mass percentage, at least the following raw materials are included: 250-260 parts of Portland cement, 1100-1200 parts of coarse aggregate, 750-800 parts of fine aggregate, 40-80 parts of mineral admixture, 1-4 parts of water reducer, 145-155 parts of water, 1-5 parts of nano-attapulgite, 5-10 parts of polyvinyl acetate emulsion, and 7-15 parts of sisal fiber; The nano attapulgite is modified by the following method: Step a: heat treating the nano-attapulgite at 200-300° C. Step b: mixing the heat-treated nano-attapulgite with dodecyltrimethylammonium chloride and water at 60-70° C., washing and drying to obtain modified nano-attapulgite; In the step b, the mass ratio of nano-attapulgite to dodecyltrimethylammonium chloride and water is 1:(0.01-0.05):(12-18).

2. The highly wear-resistant concrete specially used for steps according to claim 1 is characterized in that: The mass fraction of the nano-attapulgite is 3-5 parts, the mass fraction of the polyvinyl acetate emulsion is 7-9 parts, and the mass fraction of the sisal fiber is 10-14 parts.

3. The highly wear-resistant concrete specially used for steps according to claim 1 is characterized in that: In the step a, heat treatment is performed at 200-300° C. for 30-60 min.

4. The highly wear-resistant concrete specially used for steps according to claim 1 is characterized in that: In the step b, mixing is performed at 60-70° C. for 30-60 minutes.

5. The highly wear-resistant concrete specially used for steps according to claim 1 is characterized in that: The nano-attapulgite has a size of 50-150 nm.

6. A method for preparing highly wear-resistant concrete specifically for steps according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1: Mix silicate cement, water and mineral admixtures until uniform; Step 2: Mix the nano-attapulgite and the polyvinyl acetate emulsion until uniform to obtain a premix; Step 3: Add the premix and sisal fiber to the material in step 1 and mix until uniform; Step 4: Continue to add fine aggregate, coarse aggregate and water reducer and mix until uniform to obtain highly wear-resistant concrete.