A waterproof and flame-retardant polypropylene plastic fresh-keeping box containing graphene and sand and its preparation process

By using nitrogen-phosphorus flame-retardant cross-linking agent and graphene composite additive in polypropylene plastic, the problems of polypropylene plastic's flammability and insufficient wear resistance are solved, and high-performance waterproof, flame-retardant and wear-resistant effects are achieved, extending the Extended service life and improved safety.

CN118344671BActive Publication Date: 2024-10-29SHANDONG RUICHI MAN ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410607731.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-16
Publication Date
2024-10-29
Estimated Expiration
2044-05-16

AI Technical Summary

Technical Problem

Polypropylene plastic fresh-keeping boxes are flammable and have poor wear resistance, and existing flame retardants are very harmful to the environment and are difficult to stably exist in plastics, posing safety hazards and short service life.

Method used

Using nitrogen-phosphorus flame-retardant cross-linking agent and graphene composite additive containing graphene and sand, the flame-retardant, waterproof and wear-resistant properties of polypropylene plastic are improved through cross-linking polymerization and micro-ball effect, forming a network cross-linked structure and physical barrier layer.

Benefits of technology

It significantly improves the flame retardant performance, waterproof effect and wear resistance of polypropylene plastic fresh-keeping boxes, enhances the mechanical strength, avoids the migration and volatilization of flame retardants, extends the service life and improves safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118344671B_ABST
    Figure CN118344671B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of plastic technology, and discloses a waterproof and flame-retardant polypropylene plastic fresh-keeping box containing graphene and sand and a preparation process thereof. The plastic fresh-keeping box is made by mixing, extruding and blow molding processes with polypropylene as a base material and auxiliary materials such as nitrogen-phosphorus flame-retardant crosslinking agents and graphene composite additives. The addition of phosphorus flame-retardant crosslinking agents can improve the waterproof, flame-retardant and mechanical properties of the fresh-keeping box. The graphene composite additive, due to the lubricating effect of castor oil, can enable fine river sand to move back and forth on the surface of the graphene oxide sheet layer, and the resulting micro-ball effect can greatly improve the wear resistance of the fresh-keeping box. Moreover, under the action of a bridging agent, an organic binding layer will be formed on the surface of the graphene, which greatly increases its interface compatibility with the polypropylene matrix, so that it is evenly dispersed in the polypropylene plastic box to form a physical barrier layer, which plays a synergistic waterproof and flame-retardant effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastics, and in particular to a waterproof and flame-retardant polypropylene plastic fresh-keeping box containing graphene and sand and a preparation process thereof. Background Art

[0002] With the acceleration of the pace of modern life, fresh-keeping boxes have become an important means of storing food in daily life. In the family, fresh-keeping boxes can be used to store fruits, vegetables, meat and other foods to keep the food fresh. In restaurants and supermarkets, fresh-keeping boxes are used to display and store various foods to meet the needs of consumers. Among the many materials for fresh-keeping boxes, polypropylene stands out from the crowd with its excellent chemical resistance, heat resistance, electrical insulation and good processing performance, becoming the only choice for preparing fresh-keeping boxes. However, polypropylene itself is a flammable material with a limiting oxygen index of about 18%, and it is accompanied by melting and dripping when burning, which can easily cause the fire to spread over a large area. This makes the use of polypropylene plastic safes in areas such as kitchens have certain safety hazards. In addition, polypropylene has poor wear resistance, and it will wear and lose its fresh-keeping effect during the process of dragging back and forth. Therefore, it is urgent to develop a polypropylene plastic with excellent comprehensive performance.

[0003] By adding various functional additives to the polypropylene plastic formula, the comprehensive performance of polypropylene can be improved. For example, adding inorganic flame retardants such as aluminum hydroxide or organic halogen flame retardants can improve the flame retardant properties of polypropylene. However, inorganic flame retardants have poor flame retardant properties and generally require a large amount of addition to achieve significant effects. Organic halogen flame retardants are more harmful to the environment, and most small molecule organic flame retardants are easy to volatilize and migrate, and are difficult to stably exist in polypropylene plastics. Therefore, the present invention provides a polypropylene plastic fresh-keeping box with excellent flame retardant and other functional properties, which is highly safe and has a longer service life. Summary of the invention

[0004] 1. Technical issues to be solved

[0005] In view of the deficiencies in the prior art, the present invention provides a waterproof and flame-retardant polypropylene plastic fresh-keeping box containing graphene and sand and a preparation process thereof.

[0006] (II) Technical solution

[0007] A preparation process of a waterproof and flame-retardant polypropylene plastic fresh-keeping box containing graphene and sand, comprising the following steps:

[0008] The first step is to add polypropylene, nitrogen-phosphorus flame retardant crosslinking agent, graphene composite additive, initiator, antioxidant and lubricant into a mixer, control the temperature to 120-150°C, and mechanically stir and mix evenly to form a mixed material;

[0009] The second step is to feed the mixed material into a twin-screw extruder through a feeding port for melt extrusion, and control the temperature of each section to be 170-180°C, 180-190°C, 200-210°C, 190-200°C, 170-180°C in sequence, and adjust the screw speed to 50-60rpm, and place the masterbatch obtained by melt extrusion in a blow molding machine for blow molding to obtain a polypropylene plastic fresh-keeping box.

[0010] Preferably, the weight proportions of the raw materials in the preparation process of the fresh-keeping box are: 60-70 parts of polypropylene, 3.5-5 parts of nitrogen-phosphorus flame retardant crosslinking agent, 4-6 parts of graphene composite additive, 0.1-0.2 parts of initiator, 0.1-0.5 parts of antioxidant, and 1-2 parts of lubricant.

[0011] Preferably, the preparation method of the nitrogen-phosphorus flame retardant crosslinking agent is as follows:

[0012] The maleimide acid monomer and toluene are stirred and mixed to form a mixed liquid, and dicyclohexylcarbodiimide and N-hydroxysuccinimide are added to the mixed liquid. After the addition, mechanical stirring is performed, and activation is performed for 20-30 minutes. Nitrogen is introduced for protection. Flame retardant FRC-6 is added to the mixed liquid under ice bath conditions. After the addition, the ice bath is removed, and the mixture is stirred for 3-4 hours at room temperature. The material is discharged and purified to obtain a nitrogen-phosphorus flame retardant crosslinking agent.

[0013] Preferably, the maleimido acid monomer is any one of 3-maleimidopropionic acid, 4-maleimidobutyric acid or 6-maleimidocaproic acid.

[0014] Preferably, the molar ratio of the maleimide acid monomer to the flame retardant FRC-6 is 1:2.

[0015] Preferably, the preparation method of the graphene composite additive is as follows:

[0016] Step 1, add castor oil to anhydrous toluene, stir and mix until a uniform liquid is formed, then add a halogenated silane coupling agent and triethylamine to the liquid, after adding, turn on the heating, maintain the temperature at 60-70°C, keep stirring for 4-6 hours, cool down and discharge, and after purification, a bridging agent can be obtained;

[0017] Step 2, disperse the graphene oxide in an ethanol aqueous solution with a volume fraction of 60-70% to obtain a graphene oxide dispersion. Add fine river sand to the dispersion under continuous stirring. After the addition, ultrasonically disperse for 20-40 minutes, then add a bridging agent, and then increase the temperature to 70-80°C. After keeping warm and stirring for 4-6 hours, cool the material, wash it, and vacuum dry it to obtain a graphene composite additive.

[0018] Preferably, in Step 1, the molar ratio of castor oil to halogenated silane coupling agent is 1:1-1.5.

[0019] Preferably, in Step 1, the halogenated silane coupling agent is 3-chloropropyltriethoxysilane or (3-bromopropyl)triethoxysilane.

[0020] Preferably, in Step 2, the fine river sand is obtained by wet-milling the river sand to 2000-3000 meshes using a ball mill.

[0021] A waterproof and flame-retardant polypropylene plastic fresh-keeping box containing graphene and sand is prepared by adopting the preparation process.

[0022] (III) Beneficial technical effects

[0023] (1) The nitrogen-phosphorus flame-retardant crosslinking agent prepared by the present invention contains two equivalents of unsaturated olefinic substituents in its structure, which can undergo crosslinking polymerization with the polypropylene matrix during the subsequent melt mixing process, so that the polypropylene molecular chains are intertwined to form a mesh crosslinking structure, thereby improving the compactness of the polypropylene plastic fresh-keeping box, making it difficult for external moisture to penetrate into the fresh-keeping box, thereby showing a good waterproof effect. In addition, the nitrogen-phosphorus flame-retardant crosslinking agent is connected to the polypropylene plastic safe in the form of a chemical bond, which can not only effectively exert the nitrogen-phosphorus synergistic flame-retardant effect and enhance the flame-retardant performance of the fresh-keeping box, but also avoid the occurrence of migration and volatilization, and maintain long-term flame-retardant functionality. In addition, the nitrogen-phosphorus flame-retardant crosslinking agent structure also contains a rigid imide ring, which can also effectively enhance the mechanical strength of the fresh-keeping box.

[0024] (2) The present invention uses a bridging agent to fix fine river sand on the surface of graphene oxide sheets to prepare a graphene composite additive. Since castor oil has a lubricating effect, the fine river sand can move back and forth on the surface of the graphene oxide sheets, and the resulting micro-ball effect can greatly improve the wear resistance of the fresh-keeping box. Moreover, under the action of the bridging agent, an organic binding layer will be formed on the surface of the graphene, which greatly increases its interfacial compatibility with the polypropylene matrix, so that it is evenly dispersed in the polypropylene plastic box to form a physical barrier layer, which plays a synergistic waterproof and flame-retardant effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0026] Figure 1 This is the infrared test image of nitrogen-phosphorus flame retardant crosslinking agent;

[0027] Figure 2 This is the infrared test image of the bridging agent. DETAILED DESCRIPTION

[0028] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0029] Example 1

[0030] A waterproof and flame-retardant polypropylene plastic fresh-keeping box containing graphene and sand, comprising the following raw materials in parts by weight: 60 parts of polypropylene, 3.5 parts of nitrogen-phosphorus flame-retardant crosslinking agent, 4 parts of graphene composite additive, 0.1 parts of initiator benzoyl peroxide, 0.1 parts of antioxidant 1010, and 1 part of lubricant stearic acid;

[0031] The preparation method of the fresh-keeping box comprises the following steps:

[0032] The first step is to add polypropylene, nitrogen-phosphorus flame retardant crosslinking agent, graphene composite additive, initiator benzoyl peroxide, antioxidant 1010, and lubricant stearic acid into a mixer, control the temperature to 120° C., and mechanically stir and mix evenly to form a mixed material;

[0033] The second step is to feed the mixed material into a twin-screw extruder through a feeding port for melt extrusion, control the temperature of each section to be 175°C, 185°C, 200°C, 195°C, 175°C in sequence, and adjust the screw speed to 50rpm. Place the masterbatch obtained by melt extrusion in a blow molding machine for blow molding to obtain a polypropylene plastic fresh-keeping box.

[0034] The preparation method of the nitrogen-phosphorus flame retardant crosslinking agent is as follows:

[0035] 0.5 g of 6-maleimidocaproic acid and toluene were stirred and mixed to form a mixed solution, and dicyclohexylcarbodiimide and N-hydroxysuccinimide were added to the mixed solution. After the addition, mechanical stirring was performed, and the mixture was activated for 30 minutes. Nitrogen was introduced for protection. 1.2 g of flame retardant FRC-6 was added to the mixed solution under ice bath conditions. After the addition, the ice bath was removed, and the mixture was stirred for 3 hours at room temperature. The material was discharged and purified to obtain a nitrogen-phosphorus flame retardant crosslinking agent.

[0036] The substituted carboxyl group in the structure of 6-maleimidocaproic acid is activated by using dicyclohexylcarbodiimide and N-hydroxysuccinimide so that it can undergo an esterification condensation reaction with the flame retardant FRC-6 at room temperature. By controlling the dosage ratio of the substances, a maleimide-terminated nitrogen-phosphorus flame retardant crosslinking agent can be prepared.

[0037] Figure 1 This is the infrared test image of the nitrogen-phosphorus flame retardant crosslinking agent. As shown in the figure, 3026cm -1 The absorption peak at 1759 cm is the characteristic absorption peak of CH of the unsaturated carbon-carbon double bond in maleimide. -1 The absorption peak at 1688 cm is the characteristic absorption peak of the C=O of the ester group produced by the esterification condensation reaction. -1 The absorption peak at 1253 cm is the characteristic absorption peak of C=O of the amide group in maleimide. -1 The absorption peak that appears at is the characteristic absorption peak of O=P.

[0038] The preparation method of the graphene composite additive is as follows:

[0039] Step 1, add 1g of castor oil to anhydrous toluene, stir and mix until a uniform liquid is formed, then add 0.3g of 3-chloropropyltriethoxysilane and 0.2g of triethylamine to the liquid, after adding, turn on the heating, maintain the temperature at 65°C, keep stirring for 6h, cool and discharge, and after purification process, a bridging agent can be obtained;

[0040] Castor oil contains multiple substituted hydroxyl groups in its structure. Under the action of the alkaline catalyst triethylamine, it can react with the halogen substituents in the structure of the halosilane coupling agent 3-chloropropyltriethoxysilane. By controlling the amount of raw materials, a bridging agent containing multiple siloxane groups in its structure can be produced.

[0041] Figure 2 This is the infrared test image of the bridging agent, where 3303cm -1 The absorption peak at 1748 cm is the characteristic absorption peak of the hydroxyl groups in castor oil that did not participate in the reaction. -1 The absorption peak at 1000-1100 cm is the characteristic absorption peak of C=O of the ester group in castor oil. -1 Characteristic absorption peaks of ether bonds and silicon-oxygen bonds overlapping each other appeared.

[0042] Step 2, disperse 1.5g of graphene oxide in an ethanol aqueous solution with a volume fraction of 65% to obtain a graphene oxide dispersion. Under continuous stirring, add 0.6g of fine river sand with a particle size of 3000 mesh to the dispersion. After the addition, ultrasonically disperse for 30 minutes, then add 2.6g of a bridging agent, and then increase the temperature to 75°C. After stirring for 4 hours, cool the material, wash it, and vacuum dry it to obtain a graphene composite additive.

[0043] In a 65% ethanol aqueous solution, the siloxane groups in the bridging agent structure will hydrolyze to form silanol groups. Under high temperature conditions, these silanol groups can interact with graphene oxide and fine river sand, thereby fixing the fine river sand on the surface of graphene oxide sheets through chemical connection, forming a graphene composite additive with a special structure.

[0044] Example 2

[0045] A waterproof and flame-retardant polypropylene plastic fresh-keeping box containing graphene and sand, comprising the following raw materials in parts by weight: 65 parts of polypropylene, 4 parts of the nitrogen-phosphorus flame-retardant cross-linking agent prepared in Example 1 of the present invention, 5 parts of the graphene composite additive prepared in Example 1 of the present invention, 0.2 parts of initiator benzoyl peroxide, 0.3 parts of antioxidant 1010, and 1.5 parts of lubricant stearic acid;

[0046] The preparation method of the fresh-keeping box comprises the following steps:

[0047] The first step is to add polypropylene, the nitrogen-phosphorus flame retardant crosslinking agent prepared in Example 1 of the present invention, the graphene composite additive prepared in Example 1 of the present invention, the initiator benzoyl peroxide, the antioxidant 1010, and the lubricant stearic acid into a mixer, control the temperature to 130° C., and mechanically stir and mix evenly to form a mixed material;

[0048] The second step is to feed the mixed material into a twin-screw extruder through a feeding port for melt extrusion, control the temperature of each section to be 175°C, 185°C, 200°C, 195°C, 175°C in sequence, and adjust the screw speed to 50rpm. Place the masterbatch obtained by melt extrusion in a blow molding machine for blow molding to obtain a polypropylene plastic fresh-keeping box.

[0049] Example 3

[0050] A waterproof and flame-retardant polypropylene plastic fresh-keeping box containing graphene and sand, comprising the following raw materials in parts by weight: 70 parts of polypropylene, 5 parts of the nitrogen-phosphorus flame-retardant cross-linking agent prepared in Example 1 of the present invention, 6 parts of the graphene composite additive prepared in Example 1 of the present invention, 0.2 parts of initiator benzoyl peroxide, 0.5 parts of antioxidant 1010, and 2 parts of lubricant stearic acid;

[0051] The preparation method of the fresh-keeping box comprises the following steps:

[0052] The first step is to add polypropylene, the nitrogen-phosphorus flame retardant crosslinking agent prepared in Example 1 of the present invention, the graphene composite additive prepared in Example 1 of the present invention, the initiator benzoyl peroxide, the antioxidant 1010, and the lubricant stearic acid into a mixer, control the temperature to 150° C., and mechanically stir and mix evenly to form a mixed material;

[0053] The second step is to feed the mixed material into a twin-screw extruder through a feeding port for melt extrusion, control the temperature of each section to be 175°C, 185°C, 200°C, 195°C, 175°C in sequence, and adjust the screw speed to 50rpm. Place the masterbatch obtained by melt extrusion in a blow molding machine for blow molding to obtain a polypropylene plastic fresh-keeping box.

[0054] Comparative Example 1

[0055] A polypropylene plastic safe, which is different from Example 2 in that no nitrogen-phosphorus flame retardant cross-linking agent is added.

[0056] Comparative Example 2

[0057] A polypropylene plastic safe, which is different from Example 2 in that no graphene composite additive is added.

[0058] Comparative Example 3

[0059] A polypropylene plastic safe, which is different from Example 2 in that the graphene composite additive is replaced by graphene oxide.

[0060] Performance Testing

[0061] The polypropylene plastic safes in Examples 1 to 3 and Comparative Examples 1 to 3 were cut into test samples and subjected to performance tests:

[0062]

[0063] The water vapor permeability is tested with reference to the standard GB / T 1037-2021; the limiting oxygen index is tested with reference to the standard GB / T2406-2008; the abrasion rate is tested with reference to the standard GB / T 5478-2008; and the tensile strength is tested with reference to the standard GB / T1040.3-2006.

[0064] Analysis and test results show that the polypropylene plastic fresh-keeping box prepared by using nitrogen-phosphorus flame retardant cross-linking agent and graphene composite additive as auxiliary materials has excellent waterproof, flame retardant, wear-resistant and mechanical properties, and the two have a certain synergistic effect on enhancement.

[0065] Based on the ideal embodiment of the present invention, through the above description, relevant personnel can make various changes and modifications without departing from the technical idea of ​​the present invention. The technical scope of the present invention is not limited to the content of the specification, and the technical scope must be determined according to the scope of the technical solution.

Claims

1. A preparation process of a waterproof and flame-retardant polypropylene plastic fresh-keeping box containing graphene and sand, characterized in that: The following steps are involved: The first step is to add polypropylene, nitrogen-phosphorus flame retardant crosslinking agent, graphene composite additive, initiator, antioxidant and lubricant into a mixer, control the temperature to 120-150°C, and mechanically stir and mix evenly to form a mixed material; The second step is to feed the mixed material into a twin-screw extruder through a feeding port for melt extrusion, and control the temperature of each section to be: 170-180°C, 180-190°C, 200-210°C, 190-200°C, 170-180°C, and adjust the screw speed to 50-60rpm, and place the masterbatch obtained by melt extrusion in a blow molding machine for blow molding to obtain a polypropylene plastic fresh-keeping box; The preparation method of the nitrogen-phosphorus flame retardant crosslinking agent is as follows: The maleimide acid monomer and toluene are stirred and mixed to form a mixed solution, and then dicyclohexylcarbodiimide and N-hydroxysuccinimide are added to the mixed solution. After the addition, mechanical stirring is performed, and activation is performed for 20-30 minutes. Nitrogen is introduced for protection. Flame retardant FRC-6 is added to the mixed solution under ice bath conditions. After the addition, the ice bath is removed, and the mixture is stirred for 3-4 hours at room temperature. The mixture is discharged and purified to obtain a nitrogen-phosphorus flame retardant crosslinking agent. The preparation method of the graphene composite additive is as follows: Step 1, add castor oil to anhydrous toluene, stir and mix until a uniform liquid is formed, then add a halogenated silane coupling agent and triethylamine to the liquid, after adding, turn on the heating, maintain the temperature at 60-70°C, keep stirring for 4-6 hours, cool down and discharge, and after purification, a bridging agent can be obtained; Step 2, dispersing graphene oxide in an ethanol aqueous solution with a volume fraction of 60-70% to obtain a graphene oxide dispersion, adding fine river sand to the dispersion under continuous stirring, after addition, ultrasonically disperse for 20-40 minutes, then adding a bridging agent, and then raising the temperature to 70-80°C, keeping the temperature and stirring for 4-6 hours, cooling the material, washing, and vacuum drying to obtain a graphene composite additive; The weight proportions of the raw materials in the preparation process of the fresh-keeping box are: 60-70 parts of polypropylene, 3.5-5 parts of nitrogen-phosphorus flame retardant crosslinking agent, 4-6 parts of graphene composite additive, 0.1-0.2 parts of initiator, 0.1-0.5 parts of antioxidant, and 1-2 parts of lubricant; The molar ratio of the maleimide acid monomer to the flame retardant FRC-6 is 1:2; In step 1, the molar ratio of castor oil to halogenated silane coupling agent is 1:1-1.

5.

2. The preparation process of a waterproof and flame-retardant polypropylene plastic fresh-keeping box containing graphene and sand according to claim 1, characterized in that: The maleimidic acid monomer is any one of 3-maleimidopropionic acid, 4-maleimidobutyric acid or 6-maleimidocaproic acid.

3. The preparation process of a waterproof and flame-retardant polypropylene plastic fresh-keeping box containing graphene and sand according to claim 1, characterized in that: In Step 1, the halogenated silane coupling agent is 3-chloropropyltriethoxysilane or (3-bromopropyl)triethoxysilane.

4. The preparation process of a waterproof and flame-retardant polypropylene plastic fresh-keeping box containing graphene and sand according to claim 1, characterized in that: In step 2, the fine river sand is obtained by wet-milling the river sand to 2000-3000 meshes using a ball mill.

5. A waterproof and flame-retardant polypropylene plastic fresh-keeping box containing graphene and sand, characterized in that: The method is prepared by the preparation process as claimed in claim 1.

Citation Information

Patent Citations

  • Ethylene propylene diene monomer rubber / polypropylene composite material and preparation thereof

    CN104725729A

  • Preparation method of high-performance modified polypropylene diaphragm

    CN109888154A

  • Silylated castor oil, and curing composition containing the same

    JP1998182671A

  • Method for producing esters

    JP2005179247A