A kind of high viscosity modified asphalt and preparation method thereof
By using water reducer and crosslinking agent in high viscosity modified asphalt for alternating addition and chemical reactions, combined with antioxidants, the problem of insufficient stability of traditional asphalt is solved, the viscosity and stability of asphalt is improved, and the special High temperature thermal stability and low temperature crack resistance requirements in occasions.
Patent Information
- Application Number
- CN202410135207.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-31
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-01-31
AI Technical Summary
The random copolymer molecular chain rotation in traditional high-viscosity modified asphalt hinders the penetration of organic molecules in asphalt, resulting in poor stability and cannot meet the high-temperature thermal stability and low temperatures of airport road surfaces and bridge deck pavings. Crack resistance requirements.
Water reducing agent and crosslinking agent are used to add alternately and perform water reducing and crosslinking, and combine antioxidants to improve the viscosity and stability of asphalt and meet special uses requirements.
The viscosity and stability of asphalt are enhanced through chemical reactions, the viscosity and needle level of asphalt are improved, and the requirements of high-temperature thermal stability and low-temperature crack resistance are met. It is suitable for special occasions such as bridge deck paving.
Smart Images

Figure CN118344743B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of modified asphalt, and particularly relates to a high-viscosity modified asphalt and a preparation method thereof. Background Art
[0002] Asphalt is a dark brown complex mixture of hydrocarbons of different molecular weights and their non-metallic derivatives. It is a kind of high-viscosity organic liquid, mostly in the form of liquid or semi-solid petroleum. It has a black surface, is impermeable, and is almost insoluble in water, acetone, ether, and dilute ethanol. It is soluble in organic solvents such as carbon disulfide, carbon tetrachloride, sodium hydroxide, dichloromethane, and toluene. Asphalt is an organic gelling material that is waterproof, moisture-proof, and anti-corrosive. Asphalt can be mainly divided into three types: coal tar asphalt, petroleum asphalt, and natural asphalt.
[0003] High-viscosity modified asphalt refers to asphalt that has higher viscosity, toughness and toughness than ordinary modified asphalt. This is reflected in the parameter indicators as high viscosity and a strong needle penetration. The needle penetration is generally around 40 (0.1mm). The Japan Road Association standard stipulates that the viscosity of high-viscosity modified asphalt at 60°C should be greater than 20,000 Pa s and the needle penetration should be greater than 40.
[0004] The research on high viscosity modified asphalt in my country started relatively late, mainly based on the performance test research of high viscosity modifiers. Liu Xueliang of Wuhan University of Technology (Liu Xueliang. Preparation and Performance Research of High Viscosity Modified Asphalt [D]. Hubei: Wuhan University of Technology, 2008.) prepared high viscosity modified asphalt with HVB as the modifier, and conducted performance tests on penetration, ductility and softening point. The test results met the Japanese standard for high viscosity modified asphalt. Among them, Ni Fujian et al. of Southeast University (Ni Fujian, Qin Mian, Liu Qingquan, et al. Application Research of TPS Modifier in Drainage Asphalt Mixture [J]. Journal of Highway and Transportation Research and Development, 2004, 21(10):17-21.) studied the application of TPS modifier in drainage mixture and found that the dosage of 15% modifier was more reasonable. The temperature sensitivity of the modified asphalt decreased significantly, and the high temperature thermal stability, aging resistance and low temperature crack resistance were significantly improved, meeting the requirements of high viscosity modified asphalt H1. Gao Zhongjun (Gao Zhongjun, He Weiping. Development and application research of high-viscosity asphalt modifier [J]. Highway, 2007(1): 168-170) and others from Shenzhen Haichuan Engineering Technology Co., Ltd. conducted experimental research on SNOTPS high-viscosity asphalt modifier and concluded that the modifier is a new type of asphalt modifier with wide practicability, excellent performance and simple application method. Liang Yajun et al. (Liang Yajun, Xu Zhihong. Performance evaluation of high viscosity modified asphalt [J]. Petroleum Asphalt, 2010, 24(5):20-22.) gave a performance evaluation of high viscosity modified asphalt. SBS (styrene-butadiene-styrene block copolymer) can form an elastic network structure in asphalt, with ideal elasticity, plasticity and elongation, and is therefore a commonly used viscosity modifying material. For example, Li Kuiyong (Li Kuiyong. Research on the application of high viscosity modified asphalt in permeable asphalt mixture [J]. Theoretical Research on Urban Construction (Electronic Edition), 2012(16)) pointed out that the high viscosity modified asphalt prepared by using SBS and SBR powder and PE composite modification can meet the use requirements of waterproof asphalt pavement, and its softening point and needle penetration are greatly improved. The dosage of SBS modifier generally varies with the properties of the base asphalt: Generally speaking, there is a critical value for the SBS dosage, which is generally considered to be around 6%. By adopting a special process, the amount of SBS can be increased, so as to obtain road asphalt with better road performance; Zhu Xiang of Southeast University (Yang Wei. Research on high viscosity modified asphalt bridge deck waterproof bonding layer [D]. Jiangsu: Southeast University, 2010.) developed a high viscosity modified asphalt based on SBS for bridge deck waterproof bonding layer. Liu Yongwei and others developed a modified asphalt material composed of thermoplastic rubber, tackifier, plasticizer, binder, etc. in proportion, called SPSC.Professor Zhou Xiaolong of East China University of Science and Technology (East China University of Science and Technology. A high-performance special SBS modified asphalt and its preparation method: CN201911136365.6 [P]. 2021-02-12) used SBS additives and stabilizers as raw materials and adopted the swelling-high-speed cutting-development process to prepare high-viscosity modified asphalt. Modifiers such as C9 petroleum resin and sulfur powder were used.
[0005] High-viscosity modified asphalt was usually used on drainage pavements in the past due to its high viscosity and strong ability to adhere to stones. In recent years, road builders have paid more and more attention to the high-temperature stability of pavements, and high-viscosity modified asphalt has begun to be used in some special sections of roads, such as airport pavements and bridge decks. However, most of the existing technologies currently use SBS technology, that is, styrene, butadiene and styrene block copolymers. The principle is to use the hydrophobicity of styrene, which can be combined with the water-increasing groups in asphalt and the viscosity of polymers to improve asphalt. However, traditional random copolymers, because the rotation of their molecular chains hinders the penetration of organic molecules in the asphalt into the polymer process, cannot achieve uniform distribution, and ultimately seriously affect its stability. Summary of the invention
[0006] The present invention provides a high-viscosity modified asphalt and a preparation method thereof. A water reducer, a cross-linking agent and an antioxidant are used as added raw materials. The water reducer and the cross-linking agent are added alternately. After water reduction and cross-linking, the viscosity and stability of the asphalt can be improved to meet the use requirements of special occasions.
[0007] To achieve the above objectives, the present invention adopts the following technical solutions:
[0008] A method for preparing high-viscosity modified asphalt comprises the following steps:
[0009] Heat the asphalt to 10-50℃ above the softening point; add water reducer while stirring, first add 1 / 3~1 / 2 of the total amount of water reducer, stir for 20-40 minutes, then add 1 / 3~1 / 2 of the total amount of cross-linking agent; keep the temperature 10-20℃ above the softening point, then add 1 / 3~1 / 2 of the total amount of water reducer, stir for 20-40 minutes, then add the remaining amount of cross-linking agent, and finally add the remaining water reducer; after all the water reducer and cross-linking agent are added, stir for 20-40 minutes, add a small amount of antioxidant, mix well and solidify to obtain high-viscosity modified asphalt.
[0010] In the above steps, the water reducer molecule contains a benzene ring, a carboxyl group and another hydrophilic group R, and the carboxyl group is directly connected to the benzene ring, and the structure is:
[0011]
[0012] Among them, the hydrophilic group R is a nitro group (-NO2 ), amino (-NH 2 ), hydroxyl (-OH), aldehyde (-CHO), carboxylic acid amino (-NHCOR 2 ), sulfonyl (-SO 3 H), sulfonyl (-SO 2 R' 2 ), phosphoryl (-PO 2 R' 2 ), phosphate group (-PO 2 OH) or carboxylic acid (-OCOR' 2 ); Y is hydrogen (-H), methyl (-CH 3 ), ethyl (-C 2 H 5 ), isopropyl (-CH(CH 3 ) 2 ) or tert-butyl (-C(CH 3 ));
[0013] The water reducing agent is preferably a mixture of one or more of 5-methyl-2-nitrobenzoic acid, 3-methyl-2-nitrobenzoic acid, 3-methyl-4-nitrobenzoic acid, 5-methyl-2-aminobenzoic acid, 3-methyl-2-aminobenzoic acid, 3-methyl-4-aminobenzoic acid, 4-nitroisophthalic acid, 5-nitroisophthalic acid, 2-nitroisophthalic acid, 4-nitroisophthalic acid monomethyl ester, 5-nitroisophthalic acid monomethyl ester, and 2-nitroisophthalic acid monomethyl ester;
[0014] The crosslinking agent molecule has two groups that can undergo condensation reactions; preferably, a mixture of one or more of p-hydroxybenzoic acid, o-hydroxybenzoic acid, m-hydroxybenzoic acid, formaldehyde-phenol prepolymer, formaldehyde-urea prepolymer, formaldehyde-melamine prepolymer, p-divinylbenzene (DVB), methylenebisacrylamide, methylenebisacrylic acid, p-aminobenzoic acid, o-aminobenzoic acid, and m-aminobenzoic acid;
[0015] The antioxidant is a mixture of one or more of sodium sulfite, sodium hydrosulfite, sodium thiosulfate, sodium hypophosphite, sodium nitrite, hydroquinone, resorcinol, catechol, aniline, p-phenylenediamine, p-hydroxyisopropylbenzene, p-hydroxytert-butylbenzene, and ascorbic acid (vitamin C);
[0016] The water reducer is used in an amount of 0.1-1% of the mass of asphalt, the cross-linking agent is used in an amount of 1-5% of the mass of asphalt, and the antioxidant is used in an amount of 0.01-0.1% of the mass of asphalt.
[0017] Beneficial effects: The present invention provides a high-viscosity modified asphalt and a preparation method thereof, wherein an organic acid with a benzene ring is used as the main water reducer and a cross-linking agent is used as an auxiliary agent. The asphalt is heated to above the softening point, and the water reducer and the cross-linking agent are added alternately. At this time, the asphalt is mixed with the water reducer and the cross-linking agent to produce a complex chemical reaction. After water reduction and cross-linking, the viscosity of the asphalt can be improved to meet the needs of special occasions; an antioxidant is added to prevent oxygen in the air from breaking the molecular chain; the water reducer is a benzoic acid derivative, and due to the particularity of its molecular structure, the compound can well fix the hydrophobic molecules of the asphalt body, and the hydrophilicity can basically react with the cross-linking agent very conveniently, thereby increasing the molecular grid of each component of the asphalt and also increasing the viscosity. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The present invention is a flow chart of a method for preparing a high viscosity modified asphalt mixture;
[0019] Figure 2 Schematic diagram of the asphalt viscosity enhancement reaction pathway in the present invention. DETAILED DESCRIPTION
[0020] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments: Example 1
[0021] like Figure 1 As shown, a method for preparing high-viscosity modified asphalt comprises the following steps:
[0022] Heat 1000 g of Zhonghai 70# asphalt from road petroleum asphalt to a viscous flow state (above the softening point, about 80°C). Add 1.2 g of water reducer 5-methyl-2-nitrobenzoic acid and stir for 30 minutes. Add 1.2 g of cross-linking agent p-hydroxybenzoic acid and stir for 30 minutes. Then continue to add 1.2 g of water reducer 5-methyl-2-nitrobenzoic acid and stir for 30 minutes. Then add 1.2 g of cross-linking agent p-hydroxybenzoic acid and stir for 30 minutes. Add 1.2 g of water reducer 5-methyl-2-nitrobenzoic acid and stir for 30 minutes. Finally, add 0.5 g of antioxidant tert-butylhydroquinone and stir for 30 minutes before use. Example 2
[0023] like Figure 1 As shown, a method for preparing high-viscosity modified asphalt comprises the following steps:
[0024] Heat 1000 g of Zhonghai 70# asphalt from road petroleum asphalt to a viscous flow state (above the softening point, about 75°C). Add 1.4 g of 5-methyl-2-aminobenzoic acid as a water reducer and stir for 20 minutes. Add 1.2 g of o-hydroxybenzoic acid as a crosslinker and stir for 30 minutes. Then continue to add 1.4 g of 5-methyl-2-aminobenzoic acid as a water reducer and stir for 20 minutes. Then add 1.2 g of o-hydroxybenzoic acid as a crosslinker and stir for 20 minutes. Add 1.4 g of 5-methyl-2-aminobenzoic acid as a water reducer and stir for 30 minutes. Finally, add 0.5 g of antioxidant p-hydroxytert-butylbenzene and stir for 20 minutes before use. Example 3
[0025] like Figure 1 As shown, a method for preparing high-viscosity modified asphalt comprises the following steps:
[0026] Heat 1000 g of Zhonghai 70# asphalt from road petroleum asphalt to a viscous flow state (above the softening point, about 85°C). Add 2.5 g of water reducer 4-nitroisophthalic acid and stir for 40 minutes. Add 2.1 g of crosslinking agent formaldehyde-p-methylphenol prepolymer (degree of polymerization is 2000-3000) and stir for 40 minutes. Then continue to add 2.5 g of water reducer 4-nitroisophthalic acid, stir for 40 minutes, then add 1.4 g of crosslinking agent formaldehyde-p-methylphenol prepolymer and stir for 20 minutes. Add 1.4 g of water reducer 4-nitroisophthalic acid and stir for 30 minutes. Finally, add 0.5 g of antioxidant p-hydroxytoluene, stir for 20 minutes and set aside. Example 4
[0027] like Figure 1 As shown, a method for preparing high-viscosity modified asphalt comprises the following steps:
[0028] Heat 1000 g of Zhonghai 85# asphalt from road petroleum asphalt to a viscous flow state (above the softening point, about 90°C). Add 2.0 g of water reducing agent 4-nitroisophthalic acid monomethyl ester and stir for 30 minutes. Add 2.1 g of cross-linking agent formaldehyde-phenol prepolymer (degree of polymerization is 2500-5000) and stir for 30 minutes. Then continue to add 1.5 g of water reducing agent 4-nitroisophthalic acid monomethyl ester, stir for 30 minutes, then add 1.4 g of cross-linking agent formaldehyde-phenol prepolymer and stir for 20 minutes. Add 2.0 g of water reducing agent 4-nitroisophthalic acid monomethyl ester and stir for 40 minutes. Finally, add 0.5 g of antioxidant p-hydroxytoluene, stir for 30 minutes and set aside.
[0029] Comparative Example 1
[0030] 1000 g of road petroleum asphalt Zhonghai 70# asphalt was heated to a viscous flow state (above the softening point, about 80°C) without any treatment.
[0031] Asphalt was evaluated according to the requirements of JFG F40-2004 and the corresponding specifications or national standards, including penetration (25°C, 100 g, 5s, GB / T 4509), PI value, elongation (5°C, GB / T 4508), softening point (ring and ball method, GB / T4507), Brookfield rotational viscosity (135°C, SH / T 0739), elastic recovery (25°C, SH / T 0737), density, and thin film heating test (163°C, 5h, GB / T 5304). All performance indicators can meet the requirements of JFG F40-2004 4.6.2. The results are shown in Table 1:
[0032] Table 1 Asphalt test results
[0033]
[0034] In order to evaluate and simulate the asphalt used in the actual bridge deck pavement, the waterproof layer uses the above modified asphalt, adds 10-15mm limestone, 5-10 mm basalt crushed stone, and the aggregate is fully satisfied. The specific results are shown in Table 2:
[0035] Table 2 Asphalt mixture test results
[0036]
[0037] The results show that the asphalt and asphalt mixtures of Examples 1-4 all meet the corresponding requirements, and their Brookfield rotational viscosity increases from 0.18 Pa s before modification to 0.9-1.2 Pa s. In the above examples, an organic acid with a benzene ring is used as the main water reducer, and a cross-linking agent is used as an auxiliary. The asphalt is heated to above the softening point, and the water reducer and the cross-linking agent are added alternately. At this time, the asphalt is mixed with the water reducer and the cross-linking agent to produce a complex chemical reaction. The reaction pathway is as follows Figure 2 As shown, A and B are two groups in the cross-linking agent that can react with each other, such as hydroxyl and carboxyl or amino and carboxyl, etc., X is a group on the molecular chain of the asphalt matrix, such as a benzene ring, hydrogen, methyl, ethyl, etc., which is usually a hydrophobic group; and the definitions of R and Y are consistent with the above, that is, R is a hydrophilic group and Y is a hydrophobic group on the benzene ring; there is usually a strong interaction between R and A or B, such as hydrogen bonding; after water reduction and cross-linking, the viscosity of the asphalt can be improved.
[0038] The above are only preferred embodiments of the present invention, which cannot limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical ideas proposed by the present invention shall fall within the protection scope of the present invention.
Claims
1. A method for preparing high-viscosity modified asphalt, characterized in that: The following steps are involved: Heating the asphalt to a temperature 10-50°C above the softening point; Add water reducer while stirring, first add 1 / 3~1 / 2 of the total amount of water reducer, stir for 20-40 minutes, then add 1 / 3~1 / 2 of the total amount of cross-linking agent; Keep the temperature 10-20℃ above the softening point, then add 1 / 3~1 / 2 of the total amount of water reducer, stir for 20-40 minutes, then add the remaining amount of cross-linking agent, and finally add the remaining water reducer; after all the water reducer and cross-linking agent are added, stir for 20-40 minutes, add a trace amount of antioxidant, the amount of the water reducer is 0.1-1% of the asphalt mass, the cross-linking agent is 1-5% of the asphalt mass, and the antioxidant is 0.01-0.1% of the asphalt mass. After mixing evenly, solidify and shape to obtain high-viscosity modified asphalt, wherein the cross-linking agent molecule has two groups that can undergo condensation reaction, and the molecular structure of the water reducer is: Among them, the hydrophilic group R is nitro, amino, hydroxyl, aldehyde, carboxyamido, sulfo, sulfonyl, phosphoryl, phosphate or carboxyoxy; the hydrophobic group Y is hydrogen, methyl, ethyl, isopropyl or tert-butyl group.
2. The method for preparing high-viscosity modified asphalt according to claim 1, characterized in that: The water reducer is a mixture of one or more of 5-methyl-2-nitrobenzoic acid, 3-methyl-2-nitrobenzoic acid, 3-methyl-4-nitrobenzoic acid, 5-methyl-2-aminobenzoic acid, 3-methyl-2-aminobenzoic acid, 3-methyl-4-aminobenzoic acid, 4-nitroisophthalic acid, 5-nitroisophthalic acid, 2-nitroisophthalic acid, 4-nitroisophthalic acid monomethyl ester, 5-nitroisophthalic acid monomethyl ester, and 2-nitroisophthalic acid monomethyl ester.
3. The method for preparing high-viscosity modified asphalt according to claim 1, characterized in that: The crosslinking agent is a mixture of one or more of p-hydroxybenzoic acid, o-hydroxybenzoic acid, m-hydroxybenzoic acid, formaldehyde-phenol prepolymer, formaldehyde-urea prepolymer, formaldehyde-melamine prepolymer, p-divinylbenzene, methylenebisacrylamide, methylenebisacrylic acid, p-aminobenzoic acid, o-aminobenzoic acid, and m-aminobenzoic acid.
4. The method for preparing high-viscosity modified asphalt according to claim 1, characterized in that: The antioxidant is a mixture of one or more of sodium sulfite, sodium hydrosulfite, sodium thiosulfate, sodium hypophosphite, sodium nitrite, hydroquinone, resorcinol, catechol, aniline, p-phenylenediamine, p-hydroxyisopropylbenzene, p-hydroxytert-butylbenzene and ascorbic acid.
5. The high-viscosity modified asphalt prepared by the method according to any one of claims 1 to 4, characterized in that: The structure of the modified asphalt is: Among them, A and B are two groups in the cross-linking agent that can react with each other; X is H, CH3 or C2H5; R is a hydrophilic group, and Y is a hydrophobic group; there is a strong interaction between R and A or B.
Citation Information
Patent Citations
High performance special SBS modified asphalt and preparation method thereof
CN110845857A
High-viscosity modified pitch and preparation method thereof
CN105111757A
Modified asphalt composition
KR101583763B1
Crosslinker for modified asphalt
US20050032942A1