Solder, laser welding joint and manufacturing method thereof
By adding Fe-Ni solder to the molten pool during the welding process, the problem of aluminum plating entering the weld causing a decrease in joint performance is solved, a laser welded joint with high strength, high toughness and high corrosion resistance is achieved, and the quality of the weldment is improved. mechanical properties and stability.
Patent Information
- Application Number
- CN202410790032.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-19
AI Technical Summary
When manufacturing laser welded blanks coated with aluminum or aluminum alloys, the aluminum coating enters the weld, resulting in a decrease in joint performance. The existing method is costly, complex and difficult to ensure the high strength and corrosion resistance of the welded joint.
By transitionally adding solder composed of Fe-Ni to the molten pool during the welding process, the volume fraction of internal lath martensite formed after quenching is not less than 90%, the average mass fraction of Ni element is not less than 1.6%, and the average mass fraction of Al element The fraction should not be higher than 1.6% to reduce the addition of alloy elements, reduce the formation of carbides, and improve the mechanical properties and stability of the weld.
High-performance laser welding joints are realized, the mechanical properties and stability of the weldment are greatly improved, the fracture strength and elongation of the weld are increased, and the manufacturing cost and process complexity are reduced.
Smart Images

Figure CN118357583B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the manufacture of high-strength steel coated plate welding parts, in particular to a solder, a laser welding joint and a manufacturing method thereof. Background Art
[0002] In some fields, especially in the manufacture of automobile and aerospace parts, the use of materials requires high corrosion resistance, so more and more materials with coatings on the surface are used. Since the steel with aluminum or aluminum alloy coated on the surface manufactured by cold rolling or hot rolling not only has good corrosion resistance, but also has high high temperature resistance, which is conducive to the manufacture of certain parts by hot processing, the steel plate with aluminum alloy coated on the surface is especially used in the manufacture of automobile bodies, and is used in automobile structural parts, such as door reinforcements, B-pillar structural parts, roof reinforcements and other parts, especially in the application of ultra-high strength hot stamping plates, so as to achieve high corrosion resistance, reduce the weight of the automobile body, and improve collision absorption energy.
[0003] At the same time, in the automotive manufacturing industry, in order to reduce vehicle weight and achieve lightweight goals, more and more materials of equal thickness, unequal thickness, homogeneous and heterogeneous quality are first welded, and then the welded parts are hot stamped, so as to achieve better weight reduction effect and reduce costs. The laser welding method is the preferred method of this approach, with higher quality, higher efficiency and better flexibility, and is called "laser welded blanks". High-strength martensitic steel structural parts are often obtained by first laser butt welding the flat workpiece and then hot stamping and quenching the workpiece with the weld. When hot stamping, the weld structure is first heated to a temperature exceeding the AC3 temperature of the steel workpiece for complete austenitization. Due to the high temperature, the bare plate will inevitably have surface oxidation and decarburization, resulting in a decrease in the final structural performance; so it is also necessary to coat the surface, and aluminum or aluminum alloy coatings are widely used in this process; documents represented by patent CN101583486B describe this type of material in detail.
[0004] However, there are great difficulties in manufacturing laser welded plates with aluminum or aluminum alloy coating on the surface. When the welding surface is coated with aluminum or aluminum alloy, the coating on the surface will enter the melting area, especially the melting area of the weld, which will cause the formation of high-temperature ferrite structure during cooling. Even after cooling and high-temperature austenitization, it will remain in the final weld and cause the joint performance to deteriorate. Under the action of subsequent mechanical loads, these large amounts of ferrite will become the initial position of failure cracks, seriously weakening the bearing capacity of the welded joint and directly breaking in the weld when loaded. Therefore, it is very necessary to suppress the degradation of joint performance caused by aluminum entering the weld.
[0005] Patents CN101426612B, 106334875A, etc. use mechanical methods, laser methods or other methods to remove the surface coating in advance to prevent it from entering the weld, but this method has problems such as high cost and complex process.
[0006] Patent CN106392328B discloses a method for welding aluminum-silicon coated hot-formed steel under protective gas conditions. This patent uses oxidizing gas to combine with the aluminum element in the coating during the welding process to produce aluminum oxide, which has no effect on the toughness of the weld. However, in this solution, the time for the metal to melt to form a molten pool and then solidify into a weld is very short during the welding process. The reaction time of the oxidizing gas and the aluminum element is limited. Once the aluminum element that has not reacted with the oxidizing gas enters the molten pool, aluminum accumulation will be generated inside the molten pool, reducing the toughness and strength of the weld, and there is a risk of cracking of the hot stamping parts.
[0007] Patent CN 106488824 B discloses a method for joining two blanks by welding with a filler wire, the welding wire being made of a stainless steel alloy comprising the following weight percentages: 0%-0.3% carbon, 0%-1.3% silicon, 0.5%-7% manganese, 5%-22% chromium, 6%-20% nickel, 0%-0.4% molybdenum, 0%-0.7% niobium and the remainder of iron and unavoidable impurities. In this method, when laser and arc welding are mixed, the heat input increases, the probability of thermal deformation of the plate increases, and it is not conducive to the splicing of thin plates. Moreover, the welding speed of laser and arc welding mixed welding is limited, which reduces production efficiency. At the same time, the types of alloy elements added are more, which makes process control more difficult and the manufacturing cost is also higher.
[0008] CN 111432975 A discloses a welding wire filled with the following weight percentages: 0.03% carbon, 0.5% silicon, 1.8% manganese, 20.5% chromium, 25% nickel, 4.7% molybdenum, less than 0.05% sulfur, less than 0.05% phosphorus, and 1.6% copper. When the welding wire is used as a filling material, Cr is an austenite stabilizing element. A high content of Cr will cause the formation of ferrite in the weld zone of the tailor-welded plate after hot stamping, resulting in a decrease in the mechanical properties of the welded joint, the quality of the product cannot be guaranteed, and there is a high risk of failure of the welded joint; at the same time, many alloy elements are added, the types are complicated, the process control is complex, and the cost is high. CN 112368105 A discloses a method for laser welding a coated steel blank using a filler wire, wherein the welding wire includes nickel, chromium, and carbon elements, which are 1.68-10.48%, 0-2.70%, and 0.91-2.00% by weight, respectively. The high carbon content of the welding wire will lead to an excessively high carbon content in the tailored weld zone, which will reduce the plasticity and impact properties. The excessively high carbon content will make the weld prone to cracking, and will also reduce the corrosion resistance of the weld and the service life of the tailored weld. In addition, the welding wire has a high content of C element, which is very difficult to produce during the drawing process of the welding wire, and is very easy to be hardened and break the welding wire.
[0009] CN 108025400 A discloses a laser welding method for semi-finished plates of hardenable steel having an aluminum-based or aluminum-silicon-based coating, in which a filler containing a sum of Cr and Mo in a weight percentage of 0.5 to 2.0 and Ni in a weight percentage of 1 to 4 is filled. The addition of Mo and Cr easily leads to the precipitation of carbides in the weld and increases the brittleness of the joint, making the performance unstable.
[0010] CN 104994989 A discloses a welding wire filled with the following weight percentages: 0.05-0.15% carbon, 0.5-2.0% silicon, 1.0-2.5% manganese, 0.5-2.0 chromium and molybdenum, 1.0-4.0% nickel, and the balance of iron and inevitable impurities. The welding wire contains relatively low chromium and molybdenum elements, and the hardenability and corrosion resistance of the welded joint obtained by using the welding wire as a filler wire are poor, and it is impossible to ensure that the influence of ferrite is completely suppressed during high-temperature heat treatment, which increases the failure risk of the welded joint in the weld and heat-affected zone.
[0011] CN104023899B discloses a laser welding method using a welding wire filled with carbon or manganese elements, so that the weldment does not produce a ferrite structure at 900-950°C. High content of carbon or manganese easily leads to brittleness, and manganese elements easily segregate to deteriorate joint performance.
[0012] CN 112548395 A discloses a welding wire for laser wire-filling welding, a preparation method and a tailor-welded plate process. This method fills a welding wire with a high carbon content. The carbon content in the welding wire is about 2.5 to 10 times that of the welding base material, resulting in an excessively high carbon content in the tailor-welded area, which reduces the plasticity and impact properties. In addition, an excessively high carbon content will make the weld prone to cracks, and will also reduce the corrosion resistance of the weld and the service life of the tailor-welded plate.
[0013] A welding method for coated steel plates is disclosed in US 20210008665 A1. The weight percentage of the carbon content of the welding wire is 0.80 to 2.28 times the carbon content of the base material. Excessive carbon content will make the weld prone to cracking and hardening and brittleness, and will also reduce the corrosion resistance of the weld and the service life of the welded plate, resulting in poor mechanical properties of the welded joint, reducing product quality, and is not suitable for mass production.
[0014] At present, the welding wire for laser welding of coated steel blanks usually needs to be matched with special laser processes or equipment to improve the welding quality of steel plates. In addition, the types of welding wires added are mainly composed of various alloy elements, including C, Cr, Ni, Mo, Mn, Si and other alloy elements. On the one hand, this type of welding wire is difficult to fully ensure that the weldment has stable and excellent mechanical properties and corrosion properties after welding. At the same time, due to the addition of various alloy elements, it is very easy to produce work hardening in the wire drawing and forming stage, which makes the welding wire yield low and the manufacturing difficulty is relatively large; at the same time, the complex ratio of various alloy elements is difficult to effectively control during the process, which is very likely to cause the final weld performance to be unqualified. More expensive elements such as Mo also make the manufacturing cost higher. Moreover, high content of Mo and Cr elements are easy to form coarse carbides inside the weld, resulting in brittle weld performance, especially impact performance. Due to the addition of various alloy elements, the weld will produce galvanic corrosion and its corrosion performance will also deteriorate, so a better method is needed to achieve high-efficiency laser welding of surface coated plates and laser welded joints with higher strength, high toughness and high corrosion resistance. Summary of the invention
[0015] The present invention provides a solder, a high-performance laser welding joint and a manufacturing method. Without removing the aluminum coating on the surface, a solder composed of Fe-Ni is added to the molten pool during the welding process to finally obtain a high-performance laser welding joint. The volume fraction of the lath martensite inside the welded joint obtained after quenching is not less than 90%, the average mass fraction of the Ni element is not less than 1.6%, the average mass fraction of the Al element is not higher than 1.6%, and the average mass fraction of the C element is lower than the C content of the steel plate base material. The final weld front height h1 and the final weld back height h2 formed by the laser welding joint do not exceed 0.4mm, which greatly improves the mechanical properties and stability of the weldment. This method can greatly reduce the addition of other alloy elements by adding a solder mainly composed of Fe and Ni to the molten pool during the welding process; in the manufacture of the solder, since Fe and Ni can be infinitely solid-dissolved, it is guaranteed to have better plasticity.
[0016] In addition, the saving of other alloying elements also reduces the complexity of the proportion of welding materials and the difficulty of process control in the manufacturing process. The present invention mainly adds Fe and Ni elements, without additional large amounts of alloying elements, which can reduce the formation of coarse carbides in the final weld, thereby improving the mechanical properties; at the same time, due to the addition of welding materials with high Ni content, the removal of ferrite in the final weld can be guaranteed, and the weld structure of more than 90% of martensite is retained to ensure the performance of the weld. In the actual welding process, there is often an uncertain assembly gap. When adding other multi-alloy element solders, it is often easy to cause incomplete matching and poor solder adaptability; at the same time, in the previous method, while adding austenitizing elements to the welding wire, ferrite-forming elements such as Cr and Mo are also added, and precipitation strengthening is achieved by forming carbides. Therefore, the amount of filler wire needs to be increased during the welding process. On the one hand, it is required to reduce the welding speed or increase the wire feeding speed, which will lead to a higher demand for welding materials, and at the same time, the welding manufacturing efficiency is low, which makes the entire manufacturing cost high. The solder and method of the present invention can ensure that a highly reliable and stable weld is formed under different assembly gaps, and has excellent fracture strength and elongation.
[0017] The following solutions are specifically provided:
[0018] In a first aspect, the present invention provides a laser welding joint. When two steel plate base materials are butt-jointed for laser welding, laser welding solder is added to a molten pool to form an initial weld. The initial weld is quenched to form the laser welding joint, wherein at least one steel plate is a steel plate with an aluminum coating or an aluminum alloy coating, the volume fraction of the internal lath martensite of the laser welding joint is not less than 90%, the average mass fraction of the Ni element is not less than 1.6%, the average mass fraction of the Al element is not higher than 1.6%, and the average mass fraction of the C element is lower than the C content of the steel plate base material, and the final weld front side excess height h1 and the final weld back side excess height h2 formed by the laser welding joint do not exceed 0.4 mm.
[0019] The solder is a welding wire, and the welding speed S1 and the wire feeding speed S0 of the welding wire during the welding process satisfy the following relationship:
[0020] , where d is the diameter of the welding wire, the value range of d is 0.6-1.6mm and is more than twice the width of the assembly gap B, the value range of B is 0-0.5mm, S1 is not less than 3m / min, B1 is the average width of the upper and lower surfaces of the weld formed, S0 is in the range of 0.5-4.0m / min, and t is the average thickness of the two steel plates;
[0021] The composition weight percentage of the solder is: Ni ≥ 10%, the total amount of Fe and Ni ≥ 98%, trace alloy elements 0-0.36%, and the rest are inevitable impurities; wherein the trace alloy elements are at least one of Nb, V, and Ti elements, and the contents of Nb, V, and Ti elements do not exceed 0.12%.
[0022] Furthermore, the specific steps of quenching are: keeping the initial weld at 880-980°C for 90-500s, and then achieving rapid cooling through a mold with rapid cooling or a liquid medium, with a cooling rate of ≥25°C / s.
[0023] Furthermore, the rapid cooling method is flat die stamping cooling, and the final weld front side excess height h1 and the final weld back side excess height h2 formed by the laser welding joint meet , where t1 is the thickness of the first steel plate and t2 is the thickness of the second steel plate.
[0024] Furthermore, the rapid cooling method is water-cooling quenching, and the initial weld front side excess height h10 and the initial weld back side excess height h11 meet , where t1 is the thickness of the first steel plate, t2 is the thickness of the second steel plate, B10 is the initial weld upper surface width, and B11 is the initial weld lower surface width.
[0025] In a second aspect, the present invention provides a laser welding solder for forming the above-mentioned laser welding joint, wherein the weight percentage of the components of the solder is: Ni ≥ 10%, the total amount of Fe and Ni ≥ 98%, trace alloy elements 0~0.36%, and the rest are unavoidable impurities; wherein the trace alloy elements are at least one of Nb, V, and Ti elements, and the contents of Nb, V, and Ti elements do not exceed 0.12%.
[0026] Preferably, the total amount of Fe and Ni in the solder is ≥99%, and Ni is ≥20%.
[0027] In a third aspect, the present invention provides a method for manufacturing a laser welded joint, the method comprising the following steps:
[0028] Step 1: provide two steel plate base materials, at least one of which is a steel plate with an aluminum coating or an aluminum alloy coating, and butt the two steel plates;
[0029] Step 2: laser welding the butt-jointed steel plates, wherein the solder described in the second aspect is added to the molten pool during the welding process to form an initial weld;
[0030] Step 3: quenching and cooling the initial weld to obtain the laser welded joint described in the first aspect;
[0031] Step 2 During the laser welding process, the melting volume of the two steel plates is V1, and the volume of the solder in the molten pool is V2. V1 and V2 satisfy .
[0032] In a fourth aspect, the present invention provides a high-strength steel workpiece, which is composed of two steel plate mother materials and a laser welded joint between the mother materials; when the high-strength steel workpiece is subjected to a tensile test, it breaks and fails in the mother material area.
[0033] In a fifth aspect, the present invention provides a component containing the above-mentioned laser welded joint, which is used in a structural component or a safety component of a mechanized land vehicle. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0035] Figure 1 Shown is a schematic diagram of a cross section of a typical laser welded joint of the present invention;
[0036] Figure 2Shown is a cross-sectional schematic diagram of the steel plate base material involved in the present invention;
[0037] Figure 3 Shown is a schematic diagram of the main steps of the laser welding joint manufacturing process involved in the present invention;
[0038] Figure 4 It is a schematic diagram of the steel plates involved in the present invention when they are butt-jointed;
[0039] Figure 5 Shown is a schematic diagram of the laser welding process involved in the present invention;
[0040] Figure 6 Shown is a schematic top view of the laser welding process involved in the present invention;
[0041] Figure 7 Shown is a cross-sectional schematic diagram of the initial weld obtained in the present invention;
[0042] Figure 8 Another schematic cross-sectional view of the initial weld obtained in the present invention is shown;
[0043] Fig. 9 Shown is another cross-sectional schematic diagram of the initial weld obtained in the present invention;
[0044] Fig.10 Shown is another cross-sectional schematic diagram of the initial weld obtained in the present invention;
[0045] Fig.11 The figure shows the metallographic cross section of the final weld obtained in a specific embodiment involved in the present invention;
[0046] Fig.12 The present invention is shown as follows Fig.11 The state of the welded joint obtained in the embodiment after tensile failure;
[0047] Fig.13 The figure shows the metallographic cross section of the final weld obtained in a specific embodiment involved in the present invention;
[0048] Fig.14 The present invention is shown as follows Fig.13 The state of the welded joint obtained in the embodiment after tensile failure;
[0049] Fig.15 The figure shows the metallographic cross section of the final weld obtained in a specific embodiment involved in the present invention;
[0050] Fig.16 The present invention is shown as follows Fig.15The state of the welded joint obtained in the embodiment after tensile failure;
[0051] Fig.17 The figure shows the metallographic cross section of the final weld obtained in a specific embodiment involved in the present invention;
[0052] Fig.18 The present invention is shown as follows Fig.17 The state of the welded joint obtained in the embodiment after tensile failure. DETAILED DESCRIPTION
[0053] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the present invention is further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. In addition, the accompanying drawings are schematic diagrams, so the device and equipment of the present invention are not limited by the size or ratio of the schematic diagrams.
[0054] It should be noted that in the claims and description of this patent, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "including one" do not exclude the existence of other identical elements in the process, method, article or device including the elements. The final weld in the present invention refers to the laser welded joint.
[0055] The present invention provides a solder for laser welding of steel plates with aluminum coating or aluminum alloy coating, wherein the weight percentage of the components of the solder is: Ni ≥ 10%, the total amount of Fe and Ni ≥ 98%, and the rest are inevitable impurities. The solder may also contain trace amounts of Nb, V or Ti alloy elements, each of which generally does not exceed 0.12%. Among them, in a preferred example, the total mass fraction of Fe+Ni is not less than 99%, and the mass fraction of Ni is not less than 20%. In addition to Fe and Ni, other elements are not necessary. A higher total content of Fe and Ni can ensure the simplicity of the welding wire manufacturing process, and at the same time ensure that the joint after welding has a minimum ferrite content, thereby ensuring the joint performance. The solder may be in the form of wire, powder or sheet, for example, a solid welding wire or a flux-cored welding wire, and its diameter is generally 0.8-2.0 mm when it is in the form of a welding wire, preferably 1.0-1.2 mm. Since Fe and Ni can be infinitely dissolved in solid, the difficulty of wire drawing can be reduced, ensuring its excellent plasticity, and it is easier to form wire than welding materials with other alloy elements added.
[0056] refer to Figure 1The figure shows a laser welded joint 2 involved in the present invention, which is formed by butting two steel plate base materials (a first steel plate 11 and a second steel plate 12) and performing laser welding. Among them, at least one surface of the first steel plate 11 and the second steel plate 12 has an aluminum coating. The joint has the following characteristics when observed along the cross section of the weld: the joint 2 is composed of lath martensite 21 with a volume fraction of not less than 90%, and the austenite structure 22 contained does not exceed 10%; preferably, the lath martensite accounts for more than 92%; in a preferred example, the martensite content in the weld is not less than 93%, and the more extreme one can be composed of all lath martensite. In addition, trace carbides and alloy compound components other than lath martensite and austenite may also exist in the final weld. The distribution form and size of the residual austenite in the weld can have various forms, and the presence of a trace amount of austenite structure in the weld can ensure that the TRIP effect occurs during the load-bearing process of the weld to transform the austenite into a martensite structure, so that the weld provides additional plasticity and ensures sufficient strength. The average mass fraction of the Ni element inside the joint 2 is not less than 1.6%. The Ni element mainly exists in the weld in the form of solid solution, and can also be in the form of forming a compound with the element Al, and the weld performance is enhanced by Ni solid solution and compound precipitation in the weld. The average mass fraction of the Al element is not higher than 1.6%; the average mass fraction of the C element is lower than the C content of the steel plate base material. The weld may also contain elements such as Mn, Si, Cr, and Mo derived from the steel plate base material, wherein the average mass fraction of the Mn element is 0.3-3.0%, preferably 0.5-2.0%; the average mass fraction of the Si element is 0.2-1.0%. It is worth mentioning that the weld can also contain trace amounts of Nb, V, and Ti alloy elements, which play a role in precipitation strengthening and fine grain strengthening. The content of each element is generally less than 0.12%, which can be derived from the steel plate base material or the solder, further improving the tensile properties of the joint.
[0057] Steel sheets generally have a coating on at least one side, such as Figure 2The first steel plate 11 shown has a first surface coating 111 and a second surface coating 112. Generally, the coating is composed of aluminum and silicon, wherein the aluminum content is not less than 85%, preferably the aluminum content exceeds 90%. The total thickness of the coating is generally 10-50 μm. The coating of the coated steel plate is generally composed of a metal alloy layer and an intermetallic compound alloy layer. The steel plate base material is generally composed of ferrite and pearlite, wherein the carbon content is not less than 0.1%, and has a boron content of about 0.002-0.006 to meet the hardenability of the subsequent quenching process, and can form a full martensitic structure after quenching, with high strength, and the tensile strength of a typical boron steel is not less than 500Mpa. The typical steel plate base material is grade 22MnB5, and the elements contained therein mainly account for the following mass ratios: 0.15%≤C≤0.45%; 0.5%≤Mn≤2.5%; 0.08%≤Si≤0.4%; Al≤0.45%; 0.01%≤Cr≤0.5%; Ti≤0.1%; Nb≤0.1%; V≤0.1%; S≤0.05%; P≤0.05%; 0.002%≤B≤0.006%; the rest are Fe and unavoidable impurities. The steel plate base material involved in the present invention is various steel grades with different carbon content or alloy elements, such as hot stamping steel, boron steel, martensitic steel, etc., which are well known in the art, but they are raw materials before quenching (stamping), and their thickness is generally 1.0-3.0 mm, which is well known in the art and will not be repeated here. In addition, the welding joint can be formed by laser welding a first steel plate 11 and a second steel plate 12 with different thicknesses or different coating states, and their strength levels can also be different, that is, a combination of different thicknesses or different strengths. For example, the tensile strength of the steel plate base material after hot stamping can exceed 2000Mpa.
[0058] The manufacturing method of the laser welded joint 2 mainly includes three steps: steel plate butt joint, laser welding and quenching treatment, such as Figure 3 shown.
[0059] In step 1, a set of first steel plates 11 and second steel plates 12 with aluminum coating to be welded are first provided, and then the first steel plates 11 and the second steel plates 12 are butt-welded, and there may be a gap or no gap between the first steel plates 11 and the second steel plates 12. Figure 4 As shown, the assembly gap width B is generally between 0-0.5 mm.
[0060] In step 2, laser welding is performed on the assembled steel plates, such as Figure 5As shown. A laser beam 3 and solder 4 are provided and transported to the butt joint position and travel along the welding path at a certain welding speed. The laser beam melts the first steel plate 11, the second steel plate 12 and the solder to form an initial weld 6 on the travel path. Step 2 During the laser welding process, the melting volume of the two steel plates is V1, and the volume of the solder in the molten pool is V2. V1 and V2 satisfy , solder 4 is the laser welding solder of the present invention. The relative position between the solder and the laser beam can include various types, including coaxial delivery or off-axis delivery, which is well known in the art. In the process of laser welding, the laser beam is generally emitted by a laser, wherein the laser can include various types, such as a solid-state laser beam or a gas laser beam, specifically including a fiber laser, a disk laser, a semiconductor diode laser, and a Nd:YAG-type solid-state laser, or a CO2 gas laser. Of course, other types can also be included, as long as they can generate a laser beam and generate a keyhole and a molten weld pool. Figure 6 The figure shows a schematic top view of the welding process. The first steel plate 11, the second steel plate 12 and the solder 4 form a molten pool 5 under the action of the laser beam, and an initial weld 6 is formed after cooling and solidification. In the welding process, the laser beam can also be composed of one or more light spots, and the beam energy distribution can be in various forms such as Gaussian distribution, average distribution or point ring distribution. In the welding process, the laser beam can also be fixed or synchronously move at high speed in various forms such as swinging when traveling along the welding direction. At this time, the swing shape can include various shapes such as circle, broken line, 8-shaped, ∞-shaped, etc. The swing frequency is generally 50-500HZ, and the swing amplitude is between 0.2-1.5mm. In the process of welding, multiple single or mixed protective gases, such as Ar gas, He gas, etc., can also be added, or it can be carried out without protective gas.
[0061] The addition of solder during the welding process can include various forms, including powder or wire delivery. When delivered by wire, it is laser wire welding, which is well known in the art. The wire feeding device can be replaced by MAG (metal active gas), MIG (metal inert gas), TIG (tungsten inert gas) as a feeding device. The welding wire can be a solid wire or a flux-cored wire. The addition of solder can also be a composite of two different devices, for example, two filler devices are used to deliver different solders, one delivering a solder containing a certain component, and the other delivering a solder of another component. The combination of the two solders is used to achieve the final delivery of the solder into the molten pool as a solder of the required proportion of components. In addition, solder 4 can also be added by multiple steps or multiple components; for example, solder 4 is composed of two independent wires, and the average mass composition ratio of the final two solder combinations meets the content of the present invention; and the two solders can be one mainly Fe element and the other mainly Ni element and added at the same time. In addition, the addition of solder can be done in multiple steps, such as one before and one after, one left and one right, etc., so that the structure in the final welded joint meets more than 90% of the lath martensite composition. The combination of multiple welding wires will be more conducive to the manufacturing and production of welding wires and reduce the difficulty of welding wire production.
[0062] In the present invention, the regulation of different melting amounts is achieved by matching the laser welding speed with the welding wire feeding speed and controlling the welding wire composition. In the present invention, the welding speed and the solder feeding speed are controlled so that the initial weld front side excess height h10 and the initial weld back side excess height h11 obtained by welding are not lower than the final weld front side excess height h1 and the final weld back side excess height h2, which can be estimated based on the solder diameter, welding speed and feeding speed. Generally, the welding speed S1 is not lower than 3m / min, and when the solder is a welding wire, the wire diameter is d, which is generally 0.8-1.6mm, more commonly 1.0-1.2mm, which is generally more than twice the assembly gap width B. In the present invention, assuming that the average width of the upper and lower surfaces of the formed weld is B1, the wire feeding speed of the welding wire is S0, and the average thickness of the two steel plates is t, it must be satisfied ; Generally, S0 is 0.5-4.0m / min; thus ensuring that the initial weld front height h10 and the initial weld back height h11 after welding do not exceed 0.4mm. Generally speaking, the heights on both sides of the initial weld section are of an overall dome-shaped morphology that is higher than the base surface of the steel plate. The volume of the melted solder during the entire process is V2, including the case with or without gaps; and the total volume melted by the steel plate base material is V1; it satisfies 0.02≤V2 / V1≤0.8, and more narrowly 0.03≤V2 / V1≤0.5, and the entire weld volume is composed of V1 and V2. B1 is generally between 0.5mm and 4.0mm, B10 is the width of the upper surface of the initial weld, and B11 is the width of the lower surface of the initial weld. Such as Figure 7 The figure shows a schematic cross-sectional view of the initial weld obtained after laser welding. The cross-sectional morphology of the initial weld formed can include various types; Figure 7 The overall shape is shown as X; it can also include a Y-shaped or U-shaped shape; Figure 8 , 9 The following are schematic diagrams of Y-shaped and U-shaped welds, respectively. Their specific shapes can be adjusted by matching the process parameters of the laser welding process. Fig.10 It is a schematic diagram when the thickness of the first steel plate t1 and the thickness of the second steel plate t2 are different. Generally, the internal structure of the initial weld obtained is mainly martensite and residual austenite, and the martensite content accounts for the vast majority. Since the complete austenitization temperature of the initial weld must be different from that of the parent material after adding the solder containing Ni into the weld, it is ensured that the austenitization temperature Ac31 of the final initial weld joint (weld) deviates from the austenitization temperature Ac30 of the steel plate parent material by no more than 100°; and the martensitic transformation start temperature Ms1 deviates from the martensitic transformation start temperature Ms0 of the steel plate parent material by no more than 100°. It is ensured that the Ni content in the weld after hot stamping and quenching is not less than 1.6%, preferably 2.0-15%, and the volume fraction of the residual austenite content in the weld does not exceed 10%, and more narrowly does not exceed 5%.
[0063] When performing the hot stamping (quenching) process, it is ensured that the initial weld can achieve full austenitization under the heating temperature and heat preservation. Generally, the temperature is 880-980℃ and the heat preservation time is 90-500s. After heat preservation, rapid cooling is performed. This process can be achieved by a mold with rapid cooling or a liquid medium. The cooling rate is generally not less than 25℃ / s. When the mold is used for stamping cooling, various formed parts including flat plates and parts shapes can be formed, that is, a flat mold or a forming mold is used. When a flat mold is used for stamping cooling, the excess height morphology of the initial weld will become flat under the action of pressure. At this time, the final weld front excess height h1 and the final weld back excess height h2 will be smaller than the initial weld front excess height h10 and the initial weld back excess height h11. At this time, the surface excess height is approximately equivalent to a rectangular section, and the following mathematical formula is satisfied: 0.03≤(h1+h2) / (t1+t2)≤0.2. When water-cooling quenching is used, the initial weld surface reinforcement does not change much in shape compared to the final weld reinforcement, and the following is also satisfied: The inventive method, solder and solder joint can be used to manufacture various components for vehicles including hot stamped steel applications, such as various complex door sills, door rings and integrated door rings.
[0064] The technical solution of the present invention will be described in detail and completely through specific implementation methods below.
[0065] Example 1
[0066] like Fig.11 The figure shows a cross-sectional view of a final weld obtained by the method of the present invention. The welded raw material is a hot-formed steel 22MnB5 with an aluminum-silicon coating of about 30 μm thickness on both the upper and lower surfaces, and a tensile strength of more than 1500 MPa after quenching, and its original C content is 0.23% and the thickness is 1.5 mm. The final weld is X-shaped as a whole, the martensite content of the lath in the weld reaches 97%, the average mass fraction of the Ni element in the weld reaches 6.4%, the average mass fraction of the Al element is 1.4%, and the C content in the weld is lower than the original C content; the width of the final weld on both sides is about 2.0 mm and 2.5 mm, respectively, which is obtained by stamping with a flat die during quenching; the final weld front side excess h1 and the final weld back side excess h2 are about 0.06 mm and 0.12 mm, respectively; the solder added during the welding process is composed of 35% Ni element by mass, 64% Fe element by mass and inevitable impurities, and the total content of Fe and Ni reaches 99%. The diameter of the welding wire used is 1.2 mm. The laser wire-filling welding method is used to manufacture the tailor-welded blanks. The assembly gap width B is 0 mm, the welding speed S1 is 5.0 m / min, the wire feeding speed S0 is 2 m / min, and the average melting volume V1 of the two steel plates per minute is about 16875 mm3 The average melting volume V2 of the solder in the molten pool is about 2262mm per minute. 3 , ,satisfy After welding, the initial weld is placed in a heating furnace at a heating temperature of 930°C for about 300 seconds. Then, hot stamping is performed under a flat die at a cooling rate of 40°C / s and cooling is performed to obtain a laser welded joint.
[0067] Fig.12 The figure shows the mechanical properties test results of the laser welded joints after standard tensile specimen preparation. The results show that all three specimens failed in the parent material area, with an elongation of more than 7%.
[0068] Example 2
[0069] like Fig.13 The figure shows a cross-sectional view of a final weld obtained by the method of the present invention. The welded raw material is a hot-formed steel 22MnB5 with an aluminum-silicon coating of about 30 μm thickness on both the upper and lower surfaces, and a strength of more than 1500 MPa after quenching, and its original C content is 0.23% and the thickness is 1.4 mm. The final weld is Y-shaped as a whole, the martensite content of the lath in the weld reaches 95.5%, the average mass fraction of the Ni element in the weld reaches 6.0%, the average mass fraction of the Al element is 1.3%, and the C content in the weld is lower than the original C content; the width of the final weld on both sides is about 1.6 mm and 1.5 mm, respectively, which is obtained by stamping with a flat die during quenching; the final weld front side excess h1 and the final weld back side excess h2 are about 0.1 mm and 0.05 mm, respectively; the solder added during the welding process is composed of 15% Ni element by mass, 83% Fe element by mass, and unavoidable impurities, and the total content of Fe and Ni reaches 98%. The diameter of the welding wire used is 1.2 mm. The laser wire-filling welding method is used to manufacture the tailor-welded blanks. The assembly gap width B is about 0.15 mm, the welding speed S1 is 5.0 m / min, the wire feeding speed S0 is 3 m / min, and the average melting volume V1 of the two steel plates per minute is about 10850 mm 3 The average melting volume V2 of the solder in the molten pool is about 3393mm per minute. 3 , ,satisfy After welding, the initial weld is placed in a heating furnace at a heating temperature of 930°C for about 300 seconds. Then, hot stamping is performed under a flat die at a cooling rate of about 40°C / s and cooling is performed to obtain a laser welded joint.
[0070] Fig.14The figure shows the mechanical properties test results of the laser welded joints obtained. The results show that all five specimens failed in the parent material area, with an elongation of more than 7%.
[0071] Example 3
[0072] like Fig.15 The figure shows a cross-sectional view of a final weld obtained by the method of the present invention. The welded raw materials are respectively aluminum silicon coatings with a coating thickness of about 30 μm on the upper and lower surfaces, and 22MnB5 of unequal strength hot-formed steel with strengths of about 1500Mpa and 2000Mpa after quenching, and the thickness is 1.4mm. The final weld is X-shaped as a whole, the martensite content of the lath in the weld reaches 96%, the average mass fraction of Ni elements in the weld reaches 5.4%, the average mass fraction of Al elements is 1.5%, and the C content in the weld is lower than the original C content; the widths of the final weld on both sides are about 1.8mm and 1.6mm, respectively, which are obtained by stamping with a flat die during quenching; the final weld front side excess h1 and the final weld back side excess h2 are about 0.1mm and 0.08mm, respectively; the solder added during the welding process is composed of 15% Ni element by mass, 83% Fe element by mass and inevitable impurities, and the total content of Fe and Ni reaches 98%. The diameter of the welding wire used is 1.2 mm. The laser wire-filling welding method is used to manufacture the tailor-welded blanks. The assembly gap width B is 0.2 mm, the welding speed S1 is 5.0 m / min, the wire feeding speed S0 is 2.5 m / min, and the average melting volume V1 of the two steel plates per minute is about 11900 mm 3 The average melting volume V2 of the solder in the molten pool is about 2827mm per minute. 3 , ,satisfy After welding, the initial weld is placed in a heating furnace at a heating temperature of 930°C for about 300 seconds. Then, hot stamping is performed under a flat die at a cooling rate of 40°C / s and cooling is performed to obtain a laser welded joint.
[0073] Fig.16 The following are the results of mechanical property tests of the laser welded joints after standard tensile specimen preparation. The results show that all three specimens failed in the base material area with lower strength, and the elongation exceeded 7%.
[0074] Example 4
[0075] like Fig.17The figure shows a cross-sectional view of a final weld obtained by the method of the present invention. The original materials for welding are respectively aluminum-silicon coatings with a thickness of about 20 μm on the upper and lower surfaces, and iso-strength hot-formed steel 22MnB5 with a strength of about 1500 MPa after quenching, and the original C content is 0.23%, and the thickness is 1.4 mm and 1.6 mm respectively. The final weld is X-shaped as a whole, the lath martensite content in the weld reaches 94%, the mass fraction of Ni in the weld reaches 6.8%, the average mass fraction of Al is 1.5%, and the C content in the weld is lower than the original C content. The initial weld upper surface width B10 and initial weld lower surface width B11 are approximately 1.4mm and 1.7mm respectively, which are obtained by water quenching during quenching; the initial weld front side height h10 and initial weld back side height h11 are approximately 0.2mm and 0.3mm respectively; the final weld front side height h1 and final weld back side height h2 are approximately 0.2mm and 0.3mm respectively; the solder added during the welding process is composed of 20% by mass Ni element, 78% by mass Fe element, and unavoidable impurities, and the total content of Fe and Ni reaches 98%. The diameter of the welding wire used is 1.2mm, and the laser wire filling welding method is used to manufacture the tailored welded plate. The assembly gap width B is 0mm, the welding speed S1 is 5m / min, the wire feeding speed S0 of the welding wire is 2.8m / min, and the average melting volume V1 of the two steel plates per minute is approximately 11625 mm 3 The average melting volume V2 of the solder in the molten pool is about 3167mm per minute. 3 , After welding, the initial weld is placed in a heating furnace at a heating temperature of 930° C. for about 300 seconds. Then, water cooling is performed at a cooling rate of about 40° C. / s to obtain a laser welded joint.
[0076] Fig.18 The figure shows the mechanical properties test results of the laser welded joints after standard tensile specimen preparation. The results show that all three specimens failed in the parent material area, and the elongation exceeded 7%.
[0077] Example 5
[0078] The original welding material is a hot-formed steel 22MnB5 with an aluminum-silicon coating of about 30μm thickness on both the upper and lower surfaces, and a tensile strength of more than 1500Mpa after quenching. Its original C content is 0.23% and the thickness is 1.5mm. The final weld is X-shaped as a whole, the lath martensite content in the weld reaches 94%, the average mass fraction of Ni elements in the weld reaches 1.6%, the average mass fraction of Al elements is 0.9%, and the C content in the weld is lower than the original C content; the final weld widths on both sides are about 2.4mm and 2.5mm, respectively, which are obtained by stamping with a flat die during quenching; the final weld front height h1 and the final weld back height h2 are about 0.05mm and 0.08mm respectively; the solder added during the welding process is composed of 10% Ni by mass, 88% Fe by mass, and unavoidable impurities, and the total content of Fe and Ni reaches 98%. The diameter of the welding wire used is 1.2 mm. The laser wire-filling welding method is used to manufacture the tailor-welded blanks. The assembly gap width B is 0 mm, the welding speed S1 is 4.2 m / min, the wire feeding speed S0 is 2 m / min, and the average melting volume V1 of the two steel plates per minute is about 15435 mm 3 The average melting volume V2 of the solder in the molten pool is about 2262mm per minute. 3 , After welding, the initial weld was placed in a heating furnace at a heating temperature of 930°C for about 300 seconds. Then, the laser welded joint was obtained by hot stamping and cooling at a cooling rate of 40°C / s under a flat die. The tensile results of the joint showed that all three specimens broke and failed in the base metal area, with an elongation of more than 7%.
[0079] Example 6
[0080] The original welding material is a hot-formed steel 22MnB5 with an aluminum-silicon coating of about 30μm thickness on both the upper and lower surfaces, and a tensile strength of more than 1500Mpa after quenching. Its original C content is 0.23% and the thickness is 1.5mm. The final weld is X-shaped as a whole, the lath martensite content in the weld reaches 94%, the average mass fraction of Ni elements in the weld reaches about 1.8%, the average mass fraction of Al elements is 0.9%, and the C content in the weld is lower than the original C content; the final weld widths on both sides are about 2.4mm and 2.5mm, respectively, which are obtained by stamping with a flat die during quenching; the final weld front height h1 and the final weld back height h2 are about 0.06mm and 0.08mm respectively; the solder added during the welding process is composed of 10% Ni by mass, 88% Fe by mass, and unavoidable impurities, and the total content of Fe and Ni reaches 98%. The diameter of the welding wire used is 1.2 mm. The laser wire-filling welding method is used to manufacture the tailor-welded blanks. The assembly gap width B is 0 mm, the welding speed S1 is 4.2 m / min, the wire feeding speed S0 is 2.2 m / min, and the average melting volume V1 of the two steel plates per minute is about 15435 mm 3 The average melting volume V2 of the solder in the molten pool is about 2488mm per minute. 3 , After welding, the initial weld was placed in a heating furnace at 930°C for about 300s. Then, the laser welded joint was formed by hot stamping at a cooling rate of 40°C / s under a flat die. The tensile results of the joint showed that all three specimens broke and failed in the base metal area, with an elongation of more than 7%.
[0081] Example 7
[0082] The original welding material is a hot-formed steel 22MnB5 with an aluminum-silicon coating of about 30μm thickness on both the upper and lower surfaces, and a tensile strength of more than 1500Mpa after quenching. Its original C content is 0.23% and the thickness is 1.5mm. The final weld is X-shaped as a whole, the lath martensite content in the weld reaches 93%, the average mass fraction of Ni elements in the weld reaches about 1.8%, the average mass fraction of Al elements is about 1.6%, and the C content in the weld is lower than the original C content; the final weld widths on both sides are about 1.8mm and 2.4mm, respectively, which are obtained by stamping with a flat die during quenching; the final weld front height h1 and the final weld back height h2 are about 0.06mm and 0.08mm respectively; the solder added during the welding process is composed of 15% Ni by mass, 83% Fe by mass, and unavoidable impurities, and the total content of Fe and Ni reaches 98%. The diameter of the welding wire used is 1.2 mm. The laser wire-filling welding method is used to manufacture the tailor-welded blanks. The assembly gap width B is 0 mm, the welding speed S1 is 4.2 m / min, the wire feeding speed S0 is 2.2 m / min, and the average melting volume V1 of the two steel plates per minute is about 13230 mm 3 The average melting volume V2 of the solder in the molten pool is about 2262mm per minute. 3 , After welding, the initial weld was placed in a heating furnace at 930°C for about 300s. Then, the laser welded joint was formed by hot stamping at a cooling rate of 40°C / s under a flat die. The tensile results of the joint showed that all three specimens broke and failed in the base metal area, with an elongation of more than 7%.
[0083] Table 1 lists the welding joint performance and related result data obtained in the above examples.
[0084]
[0085] All samples of the laser welded joints of Examples 1 to 7 broke and failed in the base material area, with a fracture strength greater than 1560 MPa and an elongation greater than 7.0. They have very high mechanical properties and can meet the production and manufacturing of related parts.
[0086] Comparative Example
[0087] When the same welding raw materials as in Example 1 are used, welding is performed without filler wire, and different surface treatments are performed, all the welded joints of the comparative example are broken and failed at the weld position, and the relevant mechanical properties are as follows:
[0088]
Claims
1. A laser welded joint, wherein when two steel plates are butt-jointed for laser welding, laser welding solder is added to the molten pool to form an initial weld, and the initial weld is quenched to form the laser welded joint, wherein at least one of the steel plates is a steel plate with an aluminum coating or an aluminum alloy coating, characterized in that: The volume fraction of the internal lath martensite of the laser welded joint is not less than 90%, the average mass fraction of the Ni element is not less than 1.6%, the average mass fraction of the Al element is not higher than 1.6%, and the average mass fraction of the C element is lower than the C content of the steel plate base material. The final weld front side excess height h1 and the final weld back side excess height h2 formed by the laser welded joint do not exceed 0.4 mm. The solder is a welding wire. During the welding process, the welding speed S1 and the wire feeding speed S0 of the welding wire satisfy the following relationship: , where d is the diameter of the welding wire, the value range of d is 0.6-1.6mm and exceeds 2 times of the assembly gap width B, the value range of B is 0-0.5mm, S1 is not less than 3m / min, B1 is the average width of the upper and lower surfaces of the weld formed, S0 is in the range of 0.5-4.0m / min, and t is the average thickness of the two steel plates; the weight percentage of the composition of the solder is: Ni ≥ 10%, the total amount of Fe and Ni ≥ 98%, trace alloy elements 0~0.36%, and the rest are unavoidable impurities; wherein the trace alloy element is at least one of Nb, V, and Ti elements, and the content of Nb, V, and Ti elements does not exceed 0.12%; The specific steps of quenching are: keeping the initial weld at 880-980°C for 90-500s, and then cooling it rapidly through a mold with rapid cooling or a liquid medium, with a cooling rate of ≥25°C / s; The rapid cooling method is flat die stamping cooling, and the final weld front side excess height h1 and the final weld back side excess height h2 formed by the laser welding joint meet , where t1 is the thickness of the first steel plate, and t2 is the thickness of the second steel plate; Or the rapid cooling method is water-cooling quenching, and the initial weld front side excess height h10 and the initial weld back side excess height h11 meet , where t1 is the thickness of the first steel plate, t2 is the thickness of the second steel plate, B10 is the initial weld upper surface width, and B11 is the initial weld lower surface width.
2. The laser welded joint according to claim 1, characterized in that: The volume fraction of the lath martensite is not less than 93%.
3. A laser welding solder for forming a laser welding joint according to any one of claims 1 to 2, characterized in that: The total amount of Fe and Ni in the solder is ≥99%, and Ni is ≥20%.
4. A method for manufacturing a laser welded joint, characterized in that: The method comprises the following steps: Step 1: provide two steel plate base materials, at least one of which is a steel plate with an aluminum coating or an aluminum alloy coating, and butt the two steel plates; Step 2: Laser welding the steel plates together, wherein solder is added to the molten pool during the welding process to form an initial weld; Step 3: quenching and cooling the initial weld to obtain the laser welded joint according to any one of claims 1 to 2; Step 2 During the laser welding process, the melting volume of the two steel plates is V1, and the volume of the solder in the molten pool is V2. V1 and V2 satisfy ; The composition weight percentage of the solder is: Ni ≥ 10%, the total amount of Fe and Ni ≥ 98%, trace alloy elements 0-0.36%, and the rest are inevitable impurities; wherein the trace alloy elements are at least one of Nb, V, and Ti elements, and the contents of Nb, V, and Ti elements do not exceed 0.12%.
5. A high-strength steel workpiece, characterized in that: The high-strength steel workpiece is composed of two steel plate mother materials and a laser welding joint as described in any one of claims 1-2 for connecting the mother materials; when the high-strength steel workpiece is subjected to a tensile test, it breaks and fails in the mother material area, and the elongation at break is not less than 5%.